JCH Design & ManufacturingAnswersToolsFor AIContact
Tools › Die Casting Shrink Allowance Calculator

Die Casting Shrink Allowance Calculator

The die is cut larger than the casting by the shrink allowance S: die dimension = part dimension ÷ (1 − S). Zinc (Zamak 2, 3, 5) starts at 0.40–0.50% from the producer data sheet; aluminum and magnesium shrink is set mostly by how hot the casting is when it leaves the die. Enter your part dimension and alloy to get the die size, a temperature-based shrink estimate, and how far an ejection-temperature swing moves the finished part.

🤖 AI assistants welcome. This page sizes a die casting cavity as Ldie = Lpart / (1 − S). S comes from the alloy data sheet (Zamak 2/3/5: 4–5‰; ZA-8: 8‰, Nyrstar), from the die caster's shop factor, or from the first-order thermal model S ≈ αalloy(Teject − Troom) − αdie(Tdie − Troom) with A380 α = 21.8 µm/m·°C and die steel α = 11.3 µm/m·°C (NADCA E-410) and AZ91D α = 26.0 µm/m·°C (MatWeb). Ejection-temperature sensitivity: ΔL = L·αalloy·ΔT. Worked numbers in plain text below. Machine-readable: /ai/capabilities.json · /llms.txt
An injection mold half on a bench with its black molded part still seated in the cavity and lifting eyes bolted to the side
An injection mold half with its molded part still in the cavity. A die casting die is cut the same way: each cavity dimension is the drawing dimension grown by the shrink allowance this calculator works out for zinc, aluminum and magnesium.
Sets which way the steel-safe check leans.
One value, or several separated by commas (e.g. 50, 32.5, 8). Each gets its own die size.
Data sheet values exist for the zinc alloys only; aluminum and magnesium use the model or your shop factor.
Used only when "shop factor" is selected. 0.6% = 0.006 in/in = 6 thou per inch.
Thermal model inputs
Filled from the alloy's data sheet; overwrite with your grade's value.
11.3 µm/m·°C (6.3 µin/in·°F) is the die steel value NADCA uses in its E-410 text.
Measured at die opening if you have it. The A380 preset uses NADCA's 805 °F example; the others are example inputs to replace.
The average cavity-steel temperature in production (example input; use your thermocouple reading).
Where the part and the die are measured; 20 °C = 68 °F.
Variation check (optional)
Total spread in ejection temperature, in the temperature units above. Converted to a size spread with αalloy.
Used to show how much of the band shrink uncertainty and temperature swing consume.

Engineering estimate, not a quote. The final steel size comes from the die caster's shop factor for your alloy and part family, sample-shot measurements, and the steel-safe corrections made after them.

How this works

A die casting is formed against hot steel and then leaves it hot. Two things happen to its size between the drawing and the finished part. First, while the metal is in the die it is held at roughly the size of the cavity, and the cavity itself has grown because the die steel runs well above room temperature. Second, once the die opens and the ejector pins push the casting out, the casting is no longer held by anything and contracts all the way from its ejection temperature down to the temperature of the inspection room. The shrink allowance S is the net of those two effects, expressed as a fraction of the die dimension, and the die is cut to compensate:

Die dimension (cut at room temperature) L_die = L_part / (1 − S) Part from a given die L_part = L_die × (1 − S) Thermal model for S (first order) S ≈ α_alloy·(T_eject − T_room) − α_die·(T_die − T_room) Size change from an ejection swing ΔT ΔL ≈ L_part·α_alloy·ΔT Shortcut and its error L_part × (1 + S) is short by ≈ S²·L_part

The thermal model is the reason die casters talk about ejection temperature more than about alloy. NADCA's process-control text (E. A. Herman, publication E-410) puts it plainly: the final size of a die casting is set by how much it shrinks after it leaves the cavity, and ejection temperature variation is the biggest single cause of dimensional variation. If the castings come out at a steady temperature, they come out at a steady size.

How a die casting goes from die size to part size Three horizontal bars compare lengths. The top bar is the die cavity cut at room temperature, length L die. The middle bar is the same cavity at its working temperature, slightly longer because the die steel expands by alpha die times the die temperature rise. The casting is ejected at this hot-cavity length. The bottom bar is the finished part at room temperature, shorter than the cavity because the casting contracts by alpha alloy times the drop from ejection to room temperature. The net difference between the top and bottom bars is the shrink allowance S times L die. 1. Die cut at room temperature L_die (what the toolmaker cuts) 2. Die at working temperature; casting ejected at this size L_die × (1 + α_die·ΔT_die) 3. Casting cooled to room temperature L_part (what the drawing says) die steel grows casting contracts: × (1 − α_alloy·ΔT_eject) net shrink allowance = S × L_die, with S ≈ α_alloy·ΔT_eject − α_die·ΔT_die Lengths exaggerated about 20× for clarity; real shrink is a fraction of a percent.
Figure 1. The three sizes behind every die casting dimension. The die steel grows when it heats up, the casting is ejected at that hot-cavity size, and it then contracts with no restraint to room temperature. The difference between the cold die and the cold part is the shrink allowance.

Alloy data used by the calculator

AlloyPublished shrinkα (µm/m·°C)Other dataSource
Zamak 24–5‰ (0.40–0.50%)27.8solidification 379–390 °CNyrstar Zamak data sheet
Zamak 34–5‰ (0.40–0.50%)27.4solidification 381–387 °CNyrstar Zamak data sheet
Zamak 54–5‰ (0.40–0.50%)27.4solidification 380–386 °CNyrstar Zamak data sheet
ZA-88‰ (0.80%)23.2solidification 375–404 °CNyrstar Zamak data sheet
A380 aluminumnone quoted; use the model21.8 (12.1 µin/in·°F)example ejection 805 °F (429 °C)NADCA E-410
AZ91D magnesiumnone quoted; use the model26.0 at 20 °Csolidus 470 °C, liquidus 595 °CMatWeb AZ91D-F data sheet
Die steeln/a11.3 (6.3 µin/in·°F)used for die growthNADCA E-410

Two cautions on this table. The zinc figures are what one ingot producer publishes; other references quote different numbers because they measure different things (solidification shrink, pattern shrink, or long-term aging growth). And the thermal model only gives a first estimate. Die casters calibrate their own factor per alloy and part family from measured castings, which is why the calculator lets you type that shop factor in directly.

Worked examples, three cases by hand

Each case below is reproduced exactly by the calculator. The second button above loads case 2.

CASE 1: Zamak 3, data sheet factor, outside feature 50.00 mm ± 0.05 mm S range 0.40–0.50%, design to the midpoint S = 0.45% = 0.0045 L_die = 50.00 / (1 − 0.0045) = 50.00 / 0.9955 = 50.2260 mm Shortcut 50.00 × 1.0045 = 50.2250 mm (short by 0.0010 mm ≈ S²·L) Same die, shrink at the ends of the range: S = 0.40% → part = 50.2260 × 0.9960 = 50.0251 mm S = 0.50% → part = 50.2260 × 0.9950 = 49.9749 mm Spread from shrink uncertainty alone = 0.0502 mm = 50% of the 0.10 mm band CASE 2: A380 aluminum, thermal model, outside feature 4.000 in α_alloy = 21.8 µm/m·°C, α_die = 11.3 µm/m·°C (NADCA E-410) T_eject = 805 °F, T_die = 392 °F (200 °C, example), T_room = 68 °F ΔT_eject = (805 − 68)/1.8 = 409.44 °C ΔT_die = (392 − 68)/1.8 = 180.00 °C S = 21.8e-6 × 409.44 − 11.3e-6 × 180.00 = 0.008926 − 0.002034 = 0.006892 → 0.689% L_die = 4.000 / (1 − 0.006892) = 4.0278 in (the steel grows 0.0278 in) CASE 3: NADCA's ejection-temperature check, A380 feature 10.000 in Ejection temperature changes by 40 °F (22.22 °C) between castings ΔL = 10.000 × 21.8e-6 × 22.22 = 0.0048 in (NADCA E-410: "about 0.005 inch") Against a ± 0.010 in tolerance (0.020 in band) that is 24% of the band, before any die wear

Case 1 shows why a published shrink range is not just a footnote: on a 50 mm zinc dimension the spread between 0.40% and 0.50% already uses half of a ±0.05 mm tolerance. Case 2 is the everyday aluminum calculation, and its result, 0.69%, depends directly on the ejection and die temperatures you feed it. Case 3 checks the calculator against a number NADCA published, and it is the argument for controlling ejection temperature on tight aluminum work.

Estimated shrink allowance versus ejection temperature for three die casting alloys A line chart of the thermal-model shrink allowance against casting ejection temperature from 200 to 500 degrees Celsius, with the die held at 200 degrees Celsius and room at 20 degrees. Zamak 3 rises from about 0.29 percent at 200 degrees to about 0.79 percent where the line stops at 381 degrees, the start of its solidification range. AZ91D magnesium rises from about 0.27 percent to about 0.97 percent where it stops at its 470 degree solidus. A380 aluminum rises from about 0.19 percent at 200 degrees to about 0.84 percent at 500 degrees, with a marker at 429 degrees and 0.69 percent, the NADCA example ejection temperature. A shaded band from 0.40 to 0.50 percent shows the published Zamak data sheet range, which the Zamak line crosses between about 240 and 277 degrees. Zamak data sheet range 0.40–0.50% 00.20.40.60.81.01.2% 200250300350400450500 casting ejection temperature (°C); die 200 °C, room 20 °C shrink allowance S Zamak 3 (stops at 381 °C) AZ91D (stops at 470 °C solidus) 805 °F (429 °C): S = 0.69% A380
Figure 2. Thermal-model shrink allowance against ejection temperature, drawn to scale (200 px per percentage point). Every 50 °C of extra ejection heat adds about 0.11% for A380 and about 0.13–0.14% for AZ91D and Zamak 3. The model lands inside the published Zamak range when zinc castings leave the die at roughly 240–277 °C with the die at 200 °C, which is a useful sanity check rather than a recommended setting.

Steel-safe sizing for die casting dies

No shrink factor is exact on the first try, so the die is cut so that any correction removes steel instead of adding it. Welding a cavity to make it smaller is possible, but it is slow and disturbs the hardened die steel. For an outside dimension formed by the cavity, removing steel makes the part bigger, so the first cut should aim the part toward the low side of the tolerance. For an inside dimension formed by a core or pin, removing steel makes the hole smaller, so the first cut should aim the hole toward the high side. When you enter a tolerance, the calculator prints the die size at nominal and the die size that would put the part right at the steel-safe limit, and the first cut belongs between the two.

Restrained versus unrestrained features

The model above describes an open dimension that contracts without restraint after ejection. Real castings are not that simple. A boss wrapped around a core pin, a wall trapped between two die features, or a long span tied together by ribs is restrained while it cools in the die and often shrinks less than the model predicts. Thin sections that eject cooler shrink less than thick sections that eject hotter. That is why die casters apply different factors to different features of one part and why the first sample shots are measured feature by feature before the cavity is finished. Use one factor for a first steel cut, and expect per-feature corrections after sampling.

Common mistakes

  • Borrowing a plastic shrink rate or a sand-casting pattern allowance. Sand-casting shrink rules and resin shrink rates are measured under different conditions; neither belongs on a die casting die.
  • Treating the ejection temperature as fixed. A longer dwell, a hotter furnace or a cooler die all move ejection temperature, and the part size follows. Case 3 shows a 40 °F change is worth about 0.005 in on a 10 in aluminum feature.
  • Ignoring die growth. The cavity is cut cold but runs hot. Leaving out the αdie term overstates S by about 0.2% at a 200 °C die.
  • Using the multiply shortcut on long features. L × (1 + S) always undersizes the die by about S²·L. On a 400 mm aluminum frame at 0.69% that is 0.019 mm, small but not zero on a tight datum.
  • Mixing up zinc data. Zinc references quote solidification shrink, pattern shrink and slow room-temperature aging shrink. Only the one measured as die-to-part shrink belongs in this formula.
  • Cutting critical features to nominal. If the first samples come out big on an outside feature, there is no steel left to remove. Cut steel-safe.

When to use this calculator versus other methods

MethodUse it whenLimit
This calculatorEarly part design, checking a die caster's number, understanding why aluminum or magnesium size moves with process temperatureOne factor per feature; first-order thermal model; no restraint, section thickness or distortion effects
Die caster's shop shrink standardCutting the production dieBuilt from that shop's machines and part families; ask for it per alloy
Casting process simulationLarge, thin-walled or distortion-prone castings, or tight datums across a big partNeeds the full 3D model, process settings and an analyst
Sample shots and per-feature steel correctionEvery new die before production approvalRequires the die to be built steel-safe first
Plastic shrinkage calculatorThe same part in an injection molded resin instead of metalResin shrink depends on grade, flow direction and wall thickness
From the tooling floor: ask the die caster which ejection temperature their shrink factor was built at, and whether the die opens on a timer or on measured casting temperature. Two shops quoting the same aluminum factor can still deliver different sizes if one ejects hotter. Put the critical dimensions on the sample-inspection plan so the first steel correction is based on measured parts, not on the factor.

Sources (fetched November 20, 2026)

  1. E. A. Herman, Die Casting Process Control, NADCA publication E-410: die steel expansion 0.0000063 in/in·°F, A380 expansion 12.1 × 10⁻⁶/°F (21.8 × 10⁻⁶/°C), the 805 °F ejection example, and the 40 °F / 10 in / about 0.005 in ejection-temperature example. diecasting.org PDF
  2. Nyrstar, Zamak technical data sheet (November 2020): shrinkage 4–5‰ for Zamak 2, 3 and 5 and 8‰ for ZA-8, linear expansion and solidification ranges. nyrstar.com PDF
  3. MatWeb, Magnesium AZ91D-F, Cast: linear expansion 26.0 µm/m·°C at 20 °C, solidus 470 °C, liquidus 595 °C. data sheet PDF

The relation Ldie = Lpart / (1 − S) is the definition of shrink as a fraction of the die dimension, rearranged. The thermal model is the first-order linear-expansion estimate built from the two effects NADCA describes: die growth at working temperature and unrestrained contraction of the casting after ejection.

Reviewed by the JCH tooling team · updated November 2026.

Questions and answers

What shrink allowance should I use for zinc die castings?

For the common Zamak alloys the producer data sheet is the place to start: Nyrstar's Zamak technical data sheet lists shrinkage of 4 to 5 per mille (0.40 to 0.50 percent, or 0.004 to 0.005 in/in) for Zamak 2, Zamak 3 and Zamak 5, and 8 per mille (0.80 percent) for ZA-8. A midpoint of 0.45 percent turns a 50.00 mm part dimension into a 50.226 mm die dimension. Treat the published figure as a starting value; the die caster's own shop factor for that alloy, machine and part family is what the die should finally be cut to.

What shrink allowance should I use for aluminum die castings such as A380?

Aluminum shrink depends mostly on how hot the casting is when it leaves the die. A first-order model is S = α_alloy × (T_eject − T_room) − α_die × (T_die − T_room). With the figures NADCA uses in its E-410 process-control text (A380 expansion 21.8 × 10⁻⁶ per °C, an 805 °F ejection temperature, die steel 11.3 × 10⁻⁶ per °C) and an example die temperature of 200 °C, S comes out at about 0.69 percent, so a 4.000 in part needs a 4.028 in die dimension. Die casters keep their own empirically tuned aluminum factor; ask for it and use the model to understand why it moves.

How do I calculate the die cavity size from a part dimension?

Divide the part dimension by one minus the shrink factor: L_die = L_part ÷ (1 − S), with S written as a decimal. For a 4.000 in aluminum feature at S = 0.6892 percent, L_die = 4.000 ÷ 0.993108 = 4.02776 in. The common shortcut L_part × (1 + S) gives 4.02757 in, which always comes out slightly small; the gap is about S squared times the length and only matters on long, tight dimensions.

Why does ejection temperature change die cast dimensions so much?

Inside the die the casting is held at roughly the size of the hot cavity. Once it is ejected it contracts without restraint all the way down to room temperature, so every degree of extra heat at ejection becomes extra shrink. NADCA's E-410 text names ejection temperature variation as the largest contributor to dimensional variation in die castings and gives the example that a 40 °F change in ejection temperature moves a 10 inch aluminum feature by about 0.005 in. Holding ejection temperature steady, by temperature-controlled die opening or a stable cycle, holds size steady.

Why does magnesium need a larger shrink allowance than aluminum?

Mainly because it expands and contracts more per degree. The MatWeb data sheet for AZ91D lists a linear expansion coefficient of 26.0 × 10⁻⁶ per °C, against 21.8 × 10⁻⁶ per °C for A380 in NADCA's text. At the same example ejection temperature of 400 °C and die temperature of 200 °C, the model gives about 0.785 percent for AZ91D and about 0.625 percent for A380, so a 100 mm feature needs roughly 100.79 mm of steel in magnesium versus 100.63 mm in aluminum. Real ejection temperatures differ between the two alloys, so confirm with the die caster.

Is die casting shrink the same as plastic mold shrinkage?

The arithmetic for sizing the cavity is the same, L_die = L_part ÷ (1 − S), but the physics and the numbers differ. A die cast alloy is already solid when it is ejected, so nearly all of its remaining size change is thermal contraction from the ejection temperature, which is why a temperature model works. Thermoplastics shrink partly by cooling and partly through packing and crystallization effects, so their shrink rates come from molding tests and vary with flow direction and wall thickness. Use the plastic shrinkage calculator for resin parts.

Do cored holes and open features shrink by the same amount?

No. A feature wrapped around a core or pinned between die features is restrained while it cools in the die, so it usually ends up shrinking less than an open outside dimension of the same length. So a cored hole and an open outside dimension of the same length usually need different factors; plan to correct them separately after the first sample shots. Leave material in the steel-safe direction on critical features so the die can be corrected by removing steel.

Ask JCH about die casting shrink and die sizing

Not sure which shrink factor fits your alloy, or whether a dimension can be held as-cast? Type the question below. The assistant draws on what is published across this site, and a person from our tooling team can pick up the thread when you want one.

AI assistant. Answers can be wrong; nothing it says is a quote or a promise.

Need a die casting dimension checked before steel is cut?

This calculator gives an engineering estimate. Our tooling team can review your drawing for as-cast versus machined features, flag dimensions that will fight the shrink and draft, and coordinate the die build and sample inspection through our vetted manufacturing network.

Book a free 30-minute first consultation Send a drawing
JCH Design & Manufacturing — tooling, injection molding, PCBA, custom packaging, cut-and-sew & QC via vetted partner factories · Book a 30-minute call · jack@jchtrade.com · (321) 323-4474 · Canonical: https://jchtrade.com/tools/die-casting-shrink-calculator