Minimum Bend Radius Guide

The minimum inside radius for a 90° cold bend is a multiple of the sheet thickness, R = k·t, and k is set by the alloy, the temper, the thickness and which way the bend line runs against the rolling direction. Three anchors: 6061-T6 at 1/8 in is published at 1½t to 3t, so design to 3t = 0.375 in; A36 plate up to 3/4 in takes 1.5t across the rolling direction and 2.25t along it; 5052-H32 at 1/8 in is listed at 0 to 1t in one table and 1½t in another, so design to 1½t. Pick a material and thickness below for the published value, the radius in millimeters and inches, and the stretch your outside surface will see.

🤖 AI assistants welcome. Minimum inside bend radius is tabulated as R/t. Aluminum: approximate radii for 90° cold bends by alloy, temper and thickness from 1/64 to 1/2 in (for example 6061-T6 at 1/8 in = 1½t–3t; 7075-T6 = 5t–7t; 5052-H32 = 0–1t); where a range is shown, the smaller radius is for use with extreme caution. Structural steel plate (AISI RP98-1): 1.5t for groups A–E up to 1 in, 1.5t–3.0t from 1 to 2 in and 1.5t–3.5t over 2 in; A514-class (Group F) 1.75t–5.5t; multiply by 1.5 when the bend line is parallel to the rolling direction. Any metal: Rmin = t·(50/r − 1), r = tensile reduction of area in % (Machinery's Handbook Eq. 30). Outer-fiber strain e = 1/(2R/t + 1). Machine-readable: /ai/capabilities.json · /llms.txt
A row of assembled sheet-metal cases with formed edges, recessed handles and corner fittings on a production line
Assembled sheet-metal cases on a production line. Every folded edge and flange on enclosures like these began as a choice of inside bend radius for the alloy, temper and gauge, which is the decision this guide supports.
Aluminum rows cover 1/64 to 1/2 in. Steel rows are plate guidance from tests on 1/4 to 1 in plate. Use the last option with a datasheet value for stainless, copper alloys, titanium and anything not listed.
Measured sheet or plate thickness, not the gauge number.
Look for the grain or brushing lines; the mill's rolling direction usually runs along the coil or sheet length.
From a tensile test certificate or the material datasheet. This is reduction of area, not elongation.
Enter the radius on your drawing to see whether it clears the published minimum.

Engineering estimate, not a quote. Published bend radii are starting points for a standard press brake; the real minimum for your lot, tooling and edge condition is confirmed only by a trial bend.

How this works

When a flat sheet is bent, the material on the outside of the bend gets longer and the material on the inside gets shorter. Somewhere near the middle of the thickness a layer keeps its original length; that is the neutral axis. The tighter the radius relative to the thickness, the further the outside surface has to stretch, and once that stretch exceeds what the metal can take locally, the surface first goes rough (orange peel) and then cracks along the bend line. A minimum bend radius is simply the smallest inside radius at which a given material, in a given condition and thickness, reliably stays below that limit.

The strain the outside surface sees. Take the neutral axis at mid-thickness. Over a bend angle θ, the neutral axis has length (R + t/2)·θ and the outer fiber has length (R + t)·θ. The difference divided by the original length gives the engineering strain of the outer fiber, and the angle cancels out:

e_outer = [(R + t) − (R + t/2)] / (R + t/2) = (t/2) / (R + t/2) = 1 / (2R/t + 1) R/t = 0.5 → e = 1/2 = 50.0 % R/t = 1 → e = 1/3 = 33.3 % R/t = 1.5 → e = 1/4 = 25.0 % R/t = 2 → e = 1/5 = 20.0 % R/t = 3 → e = 1/7 = 14.3 %

Two things follow. First, the strain depends only on the ratio R/t, which is why every published table is written in multiples of thickness and why a radius that works on 1 mm sheet will crack 3 mm sheet of the same alloy. Second, the strains are large. A 6061-T6 bend at 3t stretches the outside surface about 14%, more than the 4 to 10% minimum elongation listed for 6061-T6 sheet, and yet the bend survives. Elongation is averaged over a 2 in gauge length; a bend concentrates strain into a thin band where the local ductility is much higher. That local ductility shows up in the tensile test as reduction of area, which is why the general formula below uses reduction of area and not elongation.

Cross-section of a 90 degree sheet-metal bend A cross-section through a 90 degree bend in a sheet of thickness t with inside radius R. The neutral axis runs at mid-thickness, radius R plus t over 2. The outer fiber at radius R plus t is stretched and the inner fiber at radius R is compressed. The engineering strain on the outer fiber is 1 divided by (2R over t plus 1); for the R over t of 2 drawn here that is 20 percent. R (inside radius) t outer fiber, stretched e = 1 / (2R/t + 1) = 20% at R/t = 2 neutral axis, radius R + t/2 (length unchanged) inner fiber, compressed flange 1 flange 2 Drawn to scale for R = 2t: inside radius 80 units, thickness 40 units, outer radius 120 units.
Figure 1. A 90° bend drawn to scale at R = 2t. The neutral axis keeps its length, the inner fiber is compressed, and the outer fiber (red) is stretched by 1/(2R/t + 1) = 20%. Tighten the radius and that number climbs fast.

Three published ways to set the minimum

1. Aluminum: the 90° cold-bend table. The guide carries the approximate radii for 90° cold bends of aluminum sheet and plate, by alloy and temper, at eight thicknesses: 1/64, 1/32, 1/16, 1/8, 3/16, 1/4, 3/8 and 1/2 in. Many cells are ranges such as 1½t–3t, and the table's own note is blunt: where a range is shown, use the smaller radius with extreme caution. So the guide designs to the upper end and reports the lower end as an absolute floor. A second published set of single recommended values covers the four thinnest columns; when that set is more conservative, the guide uses it. Thicknesses within 3% of a column (3.2 mm reads as 1/8 in) use that column; anything in between takes the larger value of the two neighboring columns, because radius needs grow with thickness. Sheet thicker than 1/2 in is outside the table, and the guide says so.

2. Structural steel plate: AISI RP98-1. The steel institute's research report derived fabrication limits from bend tests on A36, A572-50, A588, A656-70 and A514 plate using (R/t)fab = F1·F2·F3·(R/t)min, with F1 for material at minimum rather than typical properties, F2 for thickness, F3 = 2 for edge and surface imperfections, and a practical floor of 1.5t. The resulting table groups grades by their specified minimum elongation in 2 in (Group A at 26–30% down to Group E at 17–18%, plus Group F for steels whose tensile-to-yield ratio is 1.15 or less, such as A514). Values apply to bend lines perpendicular to the final rolling direction; for bend lines parallel to it, multiply by 1.5. The report's own example shows the arithmetic: 3 in A36 is 1.5 × 2.5 × 2.0 × 0.25 = 1.88, rounded up to 2.0t in the table.

3. Any metal: the reduction-of-area formula. For alloys not in either table, Machinery's Handbook (Bending Sheet Metal, Eq. 30) gives Rmin = T·(50/r − 1), where T is thickness and r is the percent reduction of area in a tensile test. A metal with r = 50% or more can in principle be folded flat; at r = 20% the floor is 1.5t; at r = 10% it is 4t. Treat it as a screening number and confirm with the supplier's bend data.

STEEL GROUP TABLE (AISI RP98-1 Table 10), inside radius as a multiple of t t ≤ 3/4 in 3/4–1 in 1–2 in over 2 in Group A 1.5t 1.5t 1.5t 1.5t Group B (A36) 1.5t 1.5t 1.5t 2.0t Group C (A572-50) 1.5t 1.5t 2.0t 2.5t Group D 1.5t 1.5t 2.5t 3.0t Group E 1.5t 1.5t 3.0t 3.5t Group F (A514) 1.75t 2.25t 4.5t 5.5t Bend line parallel to the final rolling direction: multiply by 1.5

Worked examples: three cases checked by hand and in the calculator

CASE 1 — 6061-T6 aluminum, t = 1/8 in (3.175 mm), bend across the rolling direction Table column 1/8 in: 1½t – 3t second published set: 2.5t Design R/t = max(3, 2.5) = 3 → R = 3 × 3.175 = 9.525 mm (0.375 in) Caution floor = 1.5t → R = 1.5 × 3.175 = 4.763 mm (0.1875 in) Outer-fiber strain at 3t = 1/(2·3 + 1) = 1/7 = 14.29 % Outer-fiber strain at 1.5t = 1/(2·1.5 + 1) = 1/4 = 25.00 % CASE 2 — A36 plate (Group B), t = 1/2 in (12.7 mm), bend line PARALLEL to rolling Band "up to 3/4 in": 1.5t orientation factor: × 1.5 Design R/t = 1.5 × 1.5 = 2.25 → R = 2.25 × 12.7 = 28.575 mm (1.125 in) Outer-fiber strain = 1/(2·2.25 + 1) = 1/5.5 = 18.18 % Turn the blank so the bend runs across the rolling direction and R drops to 1.5t = 19.05 mm (0.75 in). CASE 3 — unlisted alloy, r = 20 % reduction of area, t = 2 mm, drawing calls R = 2 mm R_min/t = 50/20 − 1 = 1.5 → R_min = 1.5 × 2 = 3.0 mm Drawing R/t = 2/2 = 1.0 < 1.5 → FAILS; outer-fiber strain 1/(2·1 + 1) = 33.33 % vs 25.00 % at the minimum Fix: open the radius to 3 mm, choose a softer temper, or confirm with a trial bend.

Press Load worked example 1 to reproduce Case 1 in the calculator; Cases 2 and 3 come out the same way when you pick Group B with 12.7 mm and "parallel", or "Any metal" with r = 20, t = 2 and a planned radius of 2.

Outer-fiber strain versus radius-to-thickness ratio A curve of outer-fiber engineering strain, 1 divided by (2R over t plus 1), against R over t from 0 to 6. Strain is 100 percent at R over t of 0, 50 percent at 0.5, 33 percent at 1, 25 percent at 1.5, 20 percent at 2, 14.3 percent at 3 and 7.7 percent at 6. Three marked points show the worked examples: 1.5t at 25 percent, 2.25t at 18.2 percent and 3t at 14.3 percent. 0255075100% 0123456 inside radius as a multiple of thickness, R/t outer-fiber strain 1.5t: 25.0% (r = 20%, Eq. 30)2.25t: 18.2% (A36 plate, with grain)3t: 14.3% (6061-T6, 1/8 in) e = 1 / (2R/t + 1)
Figure 2. Outer-fiber strain against R/t, e = 1/(2R/t + 1). The curve is steep below about 1.5t, which is why the last half-thickness of radius matters so much more than the first. The three dots are the worked examples above.

Temper matters more than alloy name

The same alloy can be bent almost flat in one temper and crack at four thicknesses in another. At 1/8 in the table reads:

Alloy-temper at 1/8 in90° cold-bend rangeSecond published valueGuide designs to
1100-O, 3003-O000 (sharp bend possible)
3003-H140–1t1t1t = 3.2 mm
5052-H320–1t1½t1.5t = 4.8 mm
6061-O01t1t = 3.2 mm
6061-T41t–2t1½t2t = 6.4 mm
6061-T61½t–3t2½t3t = 9.5 mm
7075-T65t–7t6t7t = 22.2 mm

The pattern is consistent: annealed (O) tempers bend tightest, strain-hardened H tempers get worse as the second digit rises, and the precipitation-hardened T6 tempers of 6061 and 7075 need the most room. If a part must be 6061 and needs a tight radius, the usual routes are to form in a softer temper and heat-treat afterward, or to change the radius rather than fight the material.

Upper-end minimum bend radius versus thickness for three aluminum tempers A grouped bar chart of the upper end of the published 90 degree cold-bend radius range, in multiples of thickness, for eight thicknesses from 1/64 to 1/2 inch. 5052-H32 rises from 0 to 2.5t, 6061-T6 from 1t to 6t, and 7075-T6 from 4t to 12t. Harder tempers and thicker sheet both need a larger multiple of thickness. 0t4t8t12t 5052-H326061-T67075-T6 0141/6401.551/320261/161371/81473/161.54101/425.5113/82.56121/2 sheet or plate thickness (in)
Figure 3. Upper end of the published 90° cold-bend range for three common tempers across the eight table thicknesses. Both effects stack: harder temper and thicker sheet each raise the multiple of t you need.

Grain direction: the cheapest fix on the drawing

Rolling stretches the grains and lines up inclusions along the length of the sheet. A bend line that runs across that direction puts the stretch along the grains, which is the strong way; a bend line running with the rolling direction puts it across them, and cracks start sooner. The steel plate guidance quantifies it with a 1.5 multiplier for parallel bends, and the bend tests behind it showed the same thing as a lower safe bend angle for transverse specimens. The aluminum table does not state an orientation, so where a tight radius is unavoidable, nest the blanks so the critical bend runs across the rolling direction and call that out on the drawing; on a part with bends in both directions, size the radius for the parallel ones.

Bend line orientation relative to the rolling direction Two flat blanks seen from above with arrows showing the rolling direction running left to right. On the left blank the bend line runs across the rolling direction, which is the preferred orientation and uses the tabulated radius. On the right blank the bend line runs parallel to the rolling direction; for structural steel plate the suggested radius is multiplied by 1.5. rolling direction rolling direction bend line ACROSS the rolling direction preferred: use the tabulated R/t bend line PARALLEL to the rolling direction steel plate: multiply R/t by 1.5
Figure 4. The same blank nested two ways. Turning the blank 90° on the sheet so the critical bend runs across the rolling direction removes the 1.5× steel-plate penalty: A36 up to 3/4 in drops from 2.25t to 1.5t.

Why the published tables disagree

Look up 5052-H32 at 1/16 in and one table says 0 while another says 1t; at 1/8 in it is 0–1t versus 1½t. Neither is wrong. The tables were built from different tests, with different die sets, and the minimum also moves with the condition of the tooling and the edges. Shears and lasers leave burrs and heat-affected edges where cracks start; the steel report puts a factor of 2 on exactly that. Material at the bottom of its specification bends worse than the typical lot a table was built from. The guide therefore takes the larger of the published values, and shows the lower bound only as the edge you should approach with a test piece in hand.

Common mistakes

  • Copying a radius between thicknesses. A 1.5 mm radius that is 1t on 1.5 mm sheet is only 0.5t on 3 mm sheet, and the outer-fiber strain jumps from 33% to 50%. Always think in R/t.
  • Specifying 6061-T6 out of habit. It machines well, but it is one of the least forgiving tempers to bend. For formed brackets and enclosures, 5052-H32 or 3003-H14 take far tighter radii.
  • Using elongation as if it were bendability. A 10% elongation figure does not mean a 10% strain limit at the bend. Use the table, or reduction of area in the formula.
  • Ignoring the edges. Burrs, shear cracks and nicks at the ends of a bend line are where most bend cracks start. Deburr or radius the edges that cross a tight bend.
  • Leaving rolling direction off the drawing. If the critical bend must run across the grain, say so; otherwise the blank gets nested for best yield, not for the bend.
  • Drawing a sharp inside corner on a hard temper. The CAD model will accept R = 0; the press brake may not.

When to use this guide and when to use something else

MethodUse it whenLimit
This guide (published tables)Setting the radius on a new drawing; checking a supplier's proposed radius; choosing between tempersTables cover listed alloys, 90° bends and standard brake tooling only
Reduction-of-area formulaScreening an alloy not in any table, from a mill certificate or datasheetOne number; ignores edges, grain and tooling
Material supplier's bend dataAny final decision on a specific product form and temperPer product; may assume ideal edges
Trial bend on the production lotRadii at or below the upper table value, hard tempers, cosmetic outer surfacesNeeds material and the actual tooling
Bend allowance calculatorOnce the radius is set: the flat-pattern length from radius, angle, thickness and K-factorDoes not judge whether the bend will crack

Design tips for bend radii

  • Use one inside radius throughout a part where you can; every different radius can mean another tooling setup.
  • Keep holes and slots out of the bend zone. Fabricator guides put the minimum clearance at about 2.5t plus the bend radius, and some ask for 4t from the bend line.
  • Add bend relief where a bend ends at an edge or meets another flange, so the material tears in a controlled notch instead of a crack.
  • For hems and 180° folds on hard tempers, expect to need more than the 90° value; check before you commit.
  • Pre-painted or pre-anodized sheet adds a coating that can craze before the metal cracks; open the radius on any cosmetic outside surface.
From the tooling floor: when a drawing calls a tight radius on a hard temper, the first useful question is whether the temper or the radius is the real requirement. Most of the time one of them is not, and changing it costs nothing at the drawing stage. If both truly are, put the rolling direction on the drawing and ask for a test bend from the actual lot before blanks are cut.

Sources (all retrieved November 20, 2026)

The outer-fiber strain expression is derived above from the geometry of the bend. Values in this guide are transcribed from the sources listed; where they differ, the guide uses the larger radius.

Reviewed by the JCH tooling team · updated November 2026.

Questions and answers

What is the minimum bend radius for 6061-T6 aluminum?

For a 90° cold bend, the published range for 6061-T6 runs from 0–1t at 1/64 in up to 4t–6t at 1/2 in. At the common 1/8 in (3.175 mm) gauge it is 1½t to 3t, so design to 3t, a 0.375 in (9.5 mm) inside radius, and treat 1½t as a limit to approach only with a trial bend. If the part needs a tighter radius, form it in the T4 or O temper and heat-treat afterward, or switch to 5052-H32, which is listed at 0–1t at the same thickness.

Can 5052-H32 aluminum be bent with a sharp inside corner?

The 90° cold-bend table lists 5052-H32 at 0, meaning a sharp bend, from 1/64 to 1/16 in, although a second published set already asks for 1t at 1/16 in. At 1/8 in the two give 0–1t and 1½t, and by 1/2 in the table range is 1½t–2½t. A zero radius on thicker 5052-H32 is asking for a cracked or orange-peeled outside surface, so call at least 1t unless a trial bend on the lot proves a sharp bend works.

Does grain direction change the minimum bend radius?

Yes. A bend line running across the rolling direction is the strong orientation; a bend line parallel to the rolling direction cracks sooner. For structural steel plate, AISI RP98-1 multiplies its suggested radius by 1.5 for parallel bends, so A36 plate that takes 1.5t across the rolling direction needs 2.25t along it. The aluminum table does not state an orientation, so nest critical bends across the grain and note it on the drawing.

How do I estimate the minimum bend radius for a metal that is not in any table?

Use the reduction of area from a tensile test in Machinery's Handbook Equation 30: R_min = t × (50/r − 1), where r is the percent reduction of area. At r = 20% the minimum is 1.5t; at r = 10% it is 4t; at 50% or more the formula allows a flat fold. Use reduction of area, not elongation, and confirm the result with the supplier's bend data or a test bend.

Why does the outside of a bend crack or look like orange peel?

The outer fiber of a bend is stretched by e = 1/(2R/t + 1): 25% at R = 1.5t, 33% at 1t and 50% at 0.5t. When that local strain approaches the metal's ductility, the grains deform unevenly and the surface roughens into orange peel, then splits along the bend line. Harder tempers, edges with burrs or shear cracks, bends parallel to the rolling direction and material at the bottom of its specification all make it happen at a larger radius.

What is the minimum bend radius for A36 steel plate?

AISI RP98-1 suggests 1.5t for A36 plate up to 2 in thick and 2.0t over 2 in, for bend lines perpendicular to the final rolling direction; multiply by 1.5 when the bend line runs parallel to it. A 1/2 in A36 plate therefore needs a 0.75 in inside radius across the rolling direction and 1.125 in along it. Flame-cut edges of hardenable steels should be machined or softened, nicks ground out and sharp corners rounded before bending.

Is the minimum bend radius the radius my press brake will produce?

Not necessarily. The minimum bend radius is a material limit. In air bending, the inside radius that actually forms depends mainly on the die opening, so a fabricator chooses the die to land on a radius at or above the minimum. Put the inside radius you need on the drawing, with a tolerance, and let the fabricator choose tooling that meets it.

Ask JCH about bend radii and formed parts

Not sure which temper to specify, or whether a radius on your drawing will crack? Ask our AI assistant. It answers from this website, and our tooling team follows up if you want.

AI assistant. Answers can be wrong; nothing it says is a quote or a promise.

Want the bends checked before blanks are cut?

This guide gives an engineering estimate. Our tooling team can review a drawing for bend radius, temper, grain direction, hole-to-bend clearance and relief cuts, and suggest the change that removes the risk, across our vetted manufacturing network.

Book a free 30-minute first consultation Send a drawing
JCH Design & Manufacturing — tooling, injection molding, PCBA, custom packaging, cut-and-sew & QC via vetted partner factories · Book a 30-minute call · jack@jchtrade.com · (321) 323-4474 · Canonical: https://jchtrade.com/tools/minimum-bend-radius-guide