JCH Design & ManufacturingAnswersToolsFor AIContact
Tools › Press Brake Tonnage Calculator

Press Brake Tonnage Calculator (Air Bending)

Air-bending force is F = 1.42 × UTS × L × t² ÷ V: it grows with the square of sheet thickness and falls as the V-die opening widens. Enter thickness, die opening, bend length and tensile strength to get the force in tons and kilonewtons, the load per foot of bend, and an estimate of the inside radius that die opening will give you.

🤖 AI assistants welcome. Air-bend force F = 1.42 × UTS × L × t² / V (consistent units: MPa and mm give newtons; psi and inches give pounds-force; divide lbf by 2,000 for short tons). At the 60 ksi mild-steel baseline this is about 511 × t² / V short tons per foot with t and V in inches, which matches a published 8 × t mild-steel chart within about 5%. The older 575 × t² / V rule reads 9–17% higher at 8 × t on the same chart rows. Bottoming takes 5 or more times and coining 10 or more times the air-bend force. Worked numbers below in plain text. Machine-readable: /ai/capabilities.json · /llms.txt
A press brake with sectioned upper punches, its operator seen from behind, and a pallet of formed sheet-metal trays stacked in front of the machine
A press brake in a fabrication shop, with sectioned upper punches clamped along the ram and a pallet of formed, flanged trays in front. Every flange on that pallet was one air bend whose force depended on thickness, die opening, length and tensile strength.
Switching converts the numbers already entered.
Sets the tensile strength below. Use the value on your mill test report when you have it.
11 gauge is 0.120 in; 3 mm is 0.118 in.
Leave blank to use 8 × t (10 × t above 0.5 in / 12.7 mm).
The length of the bend line along the die, not the flange height.
Tensile, not yield. 1 ksi = 6.895 MPa.
Multipliers from published press-brake guidance; bottoming and coining vary widely.
Nameplate capacity, to show how much of the machine this bend uses.
Many punches and dies carry a maximum load per foot or per meter.

Engineering estimate, not a quote. The formula is a planning number; the press builder's load limits, the tooling ratings and a test bend on your actual material decide what the machine can do.

How this works

In air bending the sheet rests on the two shoulders of a V-shaped lower die and the punch pushes it down between them without forcing it to the bottom of the V. Mechanically that is a strip loaded at its center and supported at two points a distance V apart. The force needed rises until the metal across the bend has yielded through its full thickness, peaks, and then eases as the bend continues. The press has to deliver that peak.

The formula. For a rectangular strip of length L and thickness t, the fully plastic bending moment is the flow stress times L·t²/4, and a center load on a span V produces a moment of F·V/4. Setting the two equal gives F = stress × L × t² / V. Real bends need more than that ideal because the metal work-hardens, the sheet drags over the die shoulder radii, and the effective span shrinks as the sheet wraps into the V. Published press-brake practice folds all of that into one empirical constant and uses tensile strength rather than yield, because tensile values are more consistent from batch to batch:

F = 1.42 × UTS × L × t² / V (air bending, about 90°) Metric: UTS in MPa, L, t, V in mm → F in newtons (÷ 1000 = kN, ÷ 9,806.65 = metric tons) Imperial: UTS in psi, L, t, V in in → F in lbf (÷ 2,000 = short tons) Per foot of mild steel (UTS 60,000 psi, L = 12 in): F/ft = 1.42 × 60,000 × 12 / 2,000 × t² / V = 511 × t² / V short tons per foot Bottoming ≥ 5 × F Coining ≥ 10 × F (Bystronic method factors 5.0+ and 10.0+) Inside radius (air formed) ≈ 5 × V / 32 ≈ 0.16 × V (EngineersEdge estimate; confirm with a test bend)

What the two exponents tell you. Thickness is squared, so going from 2 mm to 3 mm sheet takes 2.25 times the force on the same die. Die opening is in the denominator, so the force halves when V doubles. That is the lever most people forget: if a bend is near the limit of the press or the tooling, a wider V-die is usually the first fix, in exchange for a larger inside radius and a longer minimum flange. Bend length and tensile strength scale the force one to one, which is why a 1.5 m stainless panel can need more press than a short bracket in plate twice as thick.

Air bending cross-section on a press brake A cross-section of an air bend. A punch comes down from the top with the bending force F. The sheet of thickness t rests on the two shoulders of a V-shaped lower die whose opening between the shoulders is V. The sheet bends into the V without touching its bottom, forming an inside radius estimated at 5 × V ÷ 32. Each flange must stay on its die shoulder through the stroke, so the shortest flange grows with the die opening. The bend length L runs into the page. F punch V-die V = die opening (shoulder to shoulder) sheet, thickness t inside radius ≈ 5 × V ÷ 32 (estimate; confirm with a test bend) flange must stay on the shoulder through the stroke bend length L runs into the page
Figure 1. Air bending. The sheet spans the die shoulders like a beam and the punch loads it at the center; the bend never reaches the bottom of the V. Force scales with L × t² ÷ V, the inside radius follows the die opening, and each flange has to be long enough to stay on its shoulder through the stroke.

Checked against a published tonnage chart

The 1.42 constant was tested here against the mild-steel air-bend table published by American Machine Tools (tons per linear foot, about 90°, mild steel), fetched November 20, 2026. The calculator's per-foot result at 60 ksi is set beside the chart value and beside the older 575 × t² ÷ V rule of thumb. The first three rows are the three acceptance cases for this tool; the rest show what happens away from the recommended 8 × t die.

Thickness on V-dieV/tChart (tons/ft)This calculatorDifference575 rule
11 ga (0.120 in) on 1 in8.37.27.36+2.2%8.28 (+15.0%)
1/4 in on 2 in8.015.315.97+4.4%17.97 (+17.4%)
3/8 in on 3 in8.024.023.96−0.2%26.95 (+12.3%)
16 ga (0.060 in) on 1/2 in8.33.63.68+2.2%4.14 (+15.0%)
1/2 in on 4 in8.033.131.95−3.5%35.94 (+8.6%)
1/4 in on 1-1/4 in5.028.825.56−11.3%28.75 (−0.2%)
1/4 in on 2-1/2 in10.011.512.78+11.1%14.38 (+25.0%)
1/4 in on 4 in16.06.27.99+28.9%8.98 (+44.8%)

Two patterns stand out. Near 8 × t the 1.42 formula lands within about 5% of the chart, while the 575 rule runs 9–17% high on those same rows, which makes it a conservative screen rather than an estimate. Away from 8 × t the chart does not follow a clean 1/V curve: in narrow dies it climbs faster than the formula (the formula reads low at 5 × t), and in wide dies it falls faster (the formula reads high). The calculator flags both zones.

Tons per foot versus die opening ratio for quarter-inch mild steel A line chart of air-bending force in tons per foot against the die opening ratio V over t for 0.25 inch mild steel at 60 ksi. The calculator curve falls from about 32 tons per foot at 4 times t to about 16 at 8 times t and 8 at 16 times t. Published chart points sit at 28.8 tons at 5 times t, 22.0 at 6 times, 15.3 at 8 times, 11.5 at 10 times, 9.1 at 12 times, 7.5 at 14 times and 6.2 at 16 times. The formula and chart agree closely between 6 and 8 times t; the chart is higher at 5 times and lower above 10 times. The recommended 8 times t die is marked. 0102030 46810121416 die opening ratio V / t short tons per foot 8 × t 28.822.015.311.59.17.56.2 1.42 formula, 60 ksipublished chart
Figure 2. Force per foot for 1/4 in mild steel as the die opening changes, drawn to scale (6.5 px per ton per foot). The blue curve is this calculator; the red points are the published chart. They agree around 6–8 × t, the chart sits higher in a narrow 5 × t die, and it falls below the formula in wide dies, where the formula becomes conservative.

Worked examples

EXAMPLE A — 2.0 mm 304 stainless panel, 1,500 mm bend, V = 16 mm (8 × t), UTS = 620 MPa F = 1.42 × 620 × 1,500 × 2.0² / 16 = 1.42 × 620 × 1,500 × 4 / 16 = 330,150 N = 330.2 kN = 33.7 metric tons = 37.1 short tons Per meter: 330.2 / 1.5 = 220.1 kN/m (22.4 t/m) Inside radius ≈ 5 × 16 / 32 = 2.5 mm (estimate; stainless may form larger, so test-bend) Same panel on V = 12 mm (6 × t): 440.2 kN (+33%), radius ≈ 5 × 12 / 32 = 1.9 mm Same panel on V = 20 mm (10 × t): 264.1 kN (−20%), radius ≈ 5 × 20 / 32 = 3.1 mm Same panel in 414 MPa mild steel on V = 16: 220.5 kN — stainless takes 1.5× the force EXAMPLE B — 1/8 in (0.125) 5052-H32 aluminum, 48 in bend, V = 1 in (8 × t), UTS = 31,000 psi (specified minimum) F = 1.42 × 31,000 × 48 × 0.125² / 1 = 33,015 lbf = 16.5 short tons Per foot: 16.5 / 4 = 4.13 tons/ft Inside radius ≈ 5 × 1 / 32 = 0.16 in (estimate) EXAMPLE C — chart check: 1/4 in mild steel, 10 ft bend, V = 2 in, UTS = 60,000 psi F = 1.42 × 60,000 × 120 × 0.25² / 2 = 319,500 lbf = 159.75 short tons (15.97 tons/ft) Published chart: 15.3 tons/ft × 10 ft = 153 tons, for which the chart's own example picks a 175-ton press. The formula is 4.4% above the chart.

Example A is the kind of bend that catches people out: thin sheet, but long and in stainless. A 2 mm panel sounds light, yet at 1.5 m it needs over 30 metric tons, and narrowing the die to tighten the radius adds another third. Example B shows how little force soft aluminum needs; the issue there is the radius and cracking, not the press. Example C reproduces a published chart case and shows the formula stays slightly on the safe side at 8 × t.

Choosing the die opening: force, radius and flange move together

The die opening is the one input you choose rather than inherit, and it sets three things at once. A narrower V raises the force in proportion, gives a tighter inside radius, and allows a shorter flange. A wider V lowers the force, opens the radius and needs a longer flange. Common practice starts at about 8 × t for sheet up to roughly 1/2 in (12.7 mm) and about 10 × t above that, which is also where published charts mark their recommended cells.

In air forming the inside radius follows the die opening. The EngineersEdge reference estimates the air-formed inside radius as R = 5 × V ÷ 32, about 16% of the die opening; harder metals form a larger radius on the same die, so confirm it with a test bend. That is why a drawing that calls for a 1 mm inside radius on 3 mm mild steel cannot be air-bent on a standard 8 × t die: 5 × 24 ÷ 32 is about 3.8 mm. If the drawing radius and the die-driven radius disagree, the flat blank and the bend allowance are wrong too; the sheet metal bend allowance calculator takes the radius from this step.

The flange has to stay on the die shoulder through the whole stroke, so the shortest flange grows with the die opening, as the American Machine Tools chart notes; take the exact minimum for your die from the tooling maker's catalog. When a flange is too short for the die that the force calls for, the choices are a different part design, a different die, or a different process, not more tonnage.

Machine and tooling limits the total does not show

A press brake's nameplate rating assumes the load is spread along the bed. A short, heavy bend concentrated at the center can exceed the safe load per foot of the ram, bed or tooling even though the total is well below the rating. Two checks matter. First, compare the load per foot (or per meter) from this calculator with the maximum stamped on the punch and die; tooling makers rate their tools that way, and broken punches are the usual result of ignoring it. Second, ask the press builder for the machine's centerline or per-foot limit, because only they can state it. The calculator compares both when you enter them.

Bottoming and coining change the picture completely. Bottoming presses the sheet against the die faces and takes 5 or more times the air-bend force (Bystronic's method factor is 5.0+); coining drives the punch tip into the metal and takes about 10 times or more. Published multiplier tables also add factors for offset, hat and hemming tooling. If a print needs a coined bend, check the per-foot tooling limit before anything else.

Common mistakes

  • Using yield strength. The 1.42 constant goes with tensile strength. Plugging in a yield value under-predicts the force, because yield is well below tensile for most sheet steels and aluminum tempers.
  • Mixing units. MPa with millimeters gives newtons; psi with inches gives pounds-force. Inches with MPa gives a number that looks plausible and is wrong.
  • Forgetting the length. Tons per foot from a chart is not the job's tonnage. Multiply by the bend length, then compare with the press.
  • Reaching for a narrow die to tighten the radius. Halving V doubles the force and can push the tooling past its per-foot rating long before the press complains.
  • Using 575 × t² ÷ V and calling it an estimate. It runs 9–17% above the published chart at 8 × t. It is fine as a ceiling, not as a press-sizing number when you are near a limit.
  • Assuming every stainless or aluminum lot is typical. Tensile strength varies by temper and by mill lot. A harder lot needs more force and springs back more. Use the mill test report.

Other ways to size the bend, and when to use them

MethodUse it whenLimit
This calculator (1.42 formula)Sizing a press, checking a quote's machine choice, comparing die openings, any material with a known tensile strengthAir bending near 90° at roughly 6–10 × t; outside that band it drifts from charts
Press or tooling maker's tonnage chartMild steel on standard dies, at the shop floorOne material basis; other metals need a tensile ratio
Steel maker's bending softwareHigh-strength and wear-resistant plate where friction and punch radius matterSpecific to that maker's grades
Test bend with a load readoutClose to the machine or tooling limit, unfamiliar alloys, tight radiiNeeds the real material and tooling
Stamping tonnage calculatorBlanking, piercing or forming in a stamping die rather than a press brakeDifferent force model (shear perimeter × thickness × shear strength)
From the tooling floor: when a bracket print gives a tight inside radius on thick stock, check the force on an 8 × t die and then on the die that would actually make that radius. The gap between those two numbers tells you whether to change the radius on the drawing, change the die, or plan for bottoming, and it is a much cheaper conversation before the blanks are cut.

Sources for the method. The air-bend formula with the 1.42 constant, F = 1.42 × UTS × t² × L ÷ (1000 × V) in kN with millimeter inputs, is reproduced in the EngineersEdge press brake forming force equation. The 575 × t² ÷ V form for 60,000 psi AISI 1035 cold-rolled steel, the tensile-ratio material factor and the method factors (air 1.0, bottoming 5.0+, coining 10.0+, offset, hat and hemming tools) are from Bystronic's how to calculate press brake tonnage. The comparison chart is the American Machine Tools press brake tonnage table for mild steel, including its 1/4 in × 10 ft example. The inside-radius estimate R = 5 × V ÷ 32 is the radius formula on the same EngineersEdge page. Material presets: 60 ksi is the chart's mild-steel basis and 90 ksi its stainless conversion; A36 at 65 ksi is the test-average tensile strength in Table 2 of AISI RP98-1, Fabrication Guidelines for Cold Bending; 5052-H32 at 31 ksi and 6061-T6 at 42 ksi are the specified minimum ultimate strengths in the Aircraft Spruce aluminum plate and sheet data table. SSAB's press force guidance covers the effect of die width and punch radius on high-strength plate. All sources accessed November 20, 2026. Your mill test report governs over any preset.

Reviewed by the JCH tooling team · updated November 2026.

Questions and answers

How do you calculate press brake tonnage for air bending?

Use F = 1.42 × UTS × L × t² ÷ V, where UTS is the ultimate tensile strength, L the bend length, t the sheet thickness and V the V-die opening. With UTS in MPa and lengths in millimeters the result is in newtons; with psi and inches it is in pounds-force, and dividing by 2,000 gives short tons. For 60 ksi mild steel this works out to about 511 × t² ÷ V short tons per foot with t and V in inches. Example: 1/4 in mild steel on a 2 in die needs about 16.0 tons per foot, so a 10 ft bend needs about 160 tons.

What V-die opening should I use for my sheet thickness?

A common starting point is a die opening of about 8 times the sheet thickness for material up to roughly 1/2 in (12.7 mm), and about 10 times above that. The opening sets the force, which halves when V doubles, and it also sets the inside radius and the shortest flange. The EngineersEdge reference estimates the air-formed inside radius as R = 5 × V ÷ 32, about 16% of the die opening; harder metals form a larger radius on the same die, so confirm it with a test bend. The flange has to stay on the die shoulder through the whole stroke, so the shortest flange grows with the die opening, as the American Machine Tools chart notes; take the exact minimum for your die from the tooling maker's catalog. Pick the die from the radius and flange the drawing needs, then check the force.

How much more tonnage does stainless steel or aluminum need than mild steel?

Force scales directly with tensile strength, so multiply the mild-steel force by the ratio of tensile strengths. 304 stainless at the 90 ksi that published charts use for stainless needs about 1.5 times the force of 60 ksi mild steel on the same die. 5052-H32 aluminum at its 31 ksi specified minimum needs a little over half, and 6061-T6 at its 42 ksi specified minimum needs about 70 percent. Tensile strength varies with temper and mill lot, so use the value on the mill test report when you are near a press or tooling limit.

Why does a narrower V-die need so much more force?

The sheet spans the die shoulders like a beam loaded at its center, and the force needed to bend a beam through its full thickness goes up as the span gets shorter. In the formula V is in the denominator, so a die half as wide needs twice the force. Published charts climb even faster than that below about 6 times the thickness: for 1/4 in mild steel on a 1-1/4 in die the chart shows 28.8 tons per foot, about 13 percent above the formula. Narrow dies are where punches and dies get overloaded.

How much more force do bottoming and coining take than air bending?

Bottoming, where the sheet is pressed against the die faces, takes 5 or more times the air-bend force (Bystronic's method factor is 5.0+). Coining, where the punch tip is driven into the metal, takes 10 or more times (method factor 10.0+). Offset, hat and hemming tools carry their own multipliers. Because the force rises so steeply, check the per-foot rating of the punch and die before planning a bottomed or coined bend.

Can a short part overload a press brake even when the total tonnage is under the rating?

Yes. The nameplate tonnage assumes the load is spread along the bed. A short bend concentrated at the center puts a high load per foot on the ram, the bed and the tooling even if the total is well below the rating. Compare the tons per foot from the calculator with the maximum stamped on the punch and die, and ask the press builder for the machine's per-foot or centerline limit, because only the builder can state it.

Why do the 575 rule and the 1.42 formula give different answers?

Both have the same form, a constant times t² ÷ V for 60 ksi steel in tons per foot, but the constants differ: 575 versus about 511 for the 1.42 version. Against a published mild-steel chart at 8 times the thickness, the 1.42 formula lands within about 5 percent while the 575 rule reads about 9 to 17 percent high. The 575 rule is a conservative ceiling; the 1.42 formula is the better estimate when you are choosing between presses or dies near a limit.

Ask JCH about bending your part

Not sure whether your bend needs a bigger press, a wider die or a different radius on the drawing? Ask our AI assistant. It draws on the guidance published on this site, and a member of our tooling team can pick up the thread with you.

Automated assistant: it can be wrong, and nothing it says is a quote or a commitment.

Planning a formed sheet-metal part?

This calculator gives an engineering estimate. Our tooling team can review the drawing, check that the radii, flanges and bend sequence suit the press and dies available, and match the part to a shop in our vetted manufacturing network that already does that kind of work. Start with a free 30-minute first consultation.

Book a 30-min call Send a drawing
JCH Design & Manufacturing — tooling, injection molding, PCBA, custom packaging, cut-and-sew & QC via vetted partner factories · Book a 30-minute call · jack@jchtrade.com · (321) 323-4474 · Canonical: https://jchtrade.com/tools/press-brake-tonnage-calculator