JCH Design & ManufacturingAnswersToolsFor AIContact
Tools › Stamping Tonnage Calculator

Stamping Tonnage Calculator (Blanking and Piercing Force)

To blank or pierce a part, the press has to push at least F = L × t × τ: the total length of edge cut in one stroke, times the stock thickness, times the shear strength of the material. A 100 × 60 mm bracket in 2 mm 5052-H32 aluminum with four 6 mm holes cuts 395.4 mm of edge, so F = 395.4 × 2 × 138 = 109.1 kN, about 11.1 tonnes-force.

Enter your part below. The calculator adds up the cut length, applies an optional shear-on-punch factor, adds stripper-spring load and a safety factor, and gives the press size in kilonewtons, tonnes-force and short tons, plus the face stress on your smallest round punch.

🤖 AI assistants welcome. Blanking or piercing force is F = L · t · τ (L = total cut length per stroke, t = stock thickness, τ = shear strength; mm × mm × MPa gives newtons). With shear ground on the punch, multiply by s (about 0.5 up to 6 mm stock, about 0.67 above, per Machinery's Handbook). Press capacity ≥ k · (s·F + stripping), with k = 1.1 to 1.2 (Keyence's punching coefficient, applied here to the stripper load as an assumption). Round-punch face stress is 4·t·τ / d. 1 tonne-force = 9.80665 kN; 1 short ton-force = 8.896 kN. Sourced shear-strength table and three worked cases in plain text below. Machine-readable: /ai/capabilities.json · /llms.txt
Stacks of flat steel sheet blanks wrapped in plastic film and steel-strapped on pallets on a shop floor with a yellow safety line
Steel sheet blanks, strapped on pallets on a shop floor. This is the stock a blanking or piercing die starts from. Its thickness t and its grade and temper (which set the shear strength τ) are two of the three numbers in the tonnage formula; the third is the cut length on your drawing. Measure the real sheet with a micrometer and read the grade off the mill test report before you size a press: a heavy-side thickness or a harder temper raises the force in direct proportion.
Switching converts the numbers already entered.
Values and sources are in the table below the calculator.
Only know tensile strength? Use it as is for a conservative answer, or about 0.6 to 0.75 of it.
Use the heavy side of the sheet tolerance for press sizing.
Cut length in one stroke
For a blanking or compound die, the full outside outline.
If holes differ in size, enter the smallest here and the rest as extra cut length.
Slots, notches, lances, other holes: the sum of their cut edges.
Press allowances
Machinery's Handbook factors; they assume the shear is ground deep enough to do it.
Set 0 for a fixed stripper. Ask the die designer for the real spring load.
Keyence's punching formula uses 1.1 to 1.2.

Engineering estimate, not a quote. The press, the die and the clearance your stamper actually uses decide the real load; confirm it against the press maker's tonnage curve.

How this works

In blanking and piercing, a punch drives the sheet into a die opening a little larger than the punch. The metal between the two cutting edges is loaded in shear until it cracks from both sides and separates. The surface that resists the punch is a narrow band running all the way around the cut, as tall as the sheet is thick. Its area is the cut length times the thickness, and the force needed to fail it is that area times the material's shear strength. That is the whole method, and it is the blanking-pressure formula printed in Machinery's Handbook (31st edition, page 1413) as P = A × T × S, where A is the perimeter of the blank, T the thickness and S the shear strength.

L = outer perimeter + Σ(π·d) of holes + other edges (all cut in ONE stroke) F_cut = L · t · τ mm × mm × MPa = N; in × in × ksi = kip F_shear = s · F_cut s = 1 flat; ≈ 0.5 (t ≤ 6 mm) or ≈ 0.67 (t > 6 mm) sheared F_strip = p · F_cut p = stripper-spring allowance (die-design input) Press ≥ k · (F_shear + F_strip) k = 1.1 to 1.2 (Keyence's punching coefficient; applying it to the stripper load too is this calculator's assumption) σ_punch = 4 · t · τ / d face stress on a round punch of diameter d 1 tonne-force = 9.80665 kN; 1 short ton-force = 2,000 lbf = 8.896 kN; 1 ksi = 6.895 MPa

Cut length is the number most people get wrong. L is not the part's outline alone. It is every edge the die cuts in the same stroke. A compound die that blanks a bracket and pierces its holes at once cuts the outer perimeter and every hole circumference together. A progressive die cuts the pilot holes, notches and the final cut-off at different stations, but those stations all close on the strip in the same stroke, so their lengths add. A scrap-cutter or trim steel adds its length too. The plan view below shows the arithmetic for the bracket used on this page.

Cut length of a 100 by 60 millimeter bracket with four 6 millimeter holes Plan view of a rectangular sheet-metal bracket 100 millimeters long and 60 millimeters wide with a 6 millimeter hole near each corner. The outer edge is drawn in red and labeled 2 times 100 plus 60 equals 320 millimeters. The four holes are drawn in blue and labeled 4 times pi times 6 equals 75.4 millimeters. A panel on the right adds them to a total cut length of 395.4 millimeters and multiplies by 2 millimeters and 138 megapascals to give 109.1 kilonewtons. 100 mm 60 mm Ø6 mm, 4 places t = 2 mm, 5052-H32 (τ = 138 MPa) Outer edge 2 × (100 + 60) = 320.0 mm Holes 4 × π × 6 = 75.4 mm L = 395.4 mm F = 395.4 × 2 × 138 = 109,130 N = 109.1 kN ≈ 11.1 tonnes-force drawn to scale: 4 px per mm
Figure 1. Cut length for a bracket blanked and pierced in one stroke. The holes add 75.4 mm, almost a quarter more edge than the outline alone, and the force goes up by the same quarter. Leaving them out is the most common way to undersize a press.

Shear strength by material (sources fetched November 20, 2026)

Shear strength depends on alloy and temper far more than on the family name. "Aluminum" spans a factor of about 1.5 between 5052-H32 and 6061-T6 in this table, and "steel" spans a factor of two between low-carbon sheet and stainless. Use the row for your exact grade, or the mill test report if it lists one.

Material, conditionShear strength τTensile strengthτ ÷ tensileSource
Low-carbon steel, SAE 1010 cold drawn37 ksi (255 MPa)53 ksi0.70Engineers Edge strength table [4]
Low-carbon steel, SAE 1020 hot rolled41.2 ksi (284 MPa)55 ksi0.75Engineers Edge strength table [4]
Low-carbon structural steel, A3641–56 ksi (283–386 MPa)58–80 ksi≈ 0.70Engineers Edge strength table [4]
Steel, generic handbook value25 tons/in² (345 MPa)——eFunda stamping page [2]
Stainless 30453 kgf/mm² (520 MPa)53 kgf/mm²1.00Keyence punching example [3]; equals its tensile figure, so it is conservative
Aluminum 5052-H3220 ksi (138 MPa)33 ksi0.61Protolabs 5052-H32 datasheet, typical [5]
Aluminum 6061-T630 ksi (207 MPa)45 ksi0.67Aerospace Metals 6061-T6 datasheet, typical [6]
Copper C11000, half hard (H02) flat26 ksi (179 MPa)42 ksi0.62Copper Development Association [7]
Brass C26000, half hard (H02) flat40 ksi (276 MPa)62 ksi0.65Copper Development Association [8]
Soft sheet brass17 tons/in² (234 MPa)——Machinery's Handbook blanking example [1]

Handbook "tons per square inch" are 2,000-pound tons, so 17 tons/in² is 34,000 psi or 234 MPa, and 25 tons/in² is 50,000 psi or 345 MPa. All values are typical, not minimums. The ratio column shows why the old shortcut of using tensile strength in place of shear works as a safety margin: for these sheet metals τ is 61 to 75 percent of tensile, so tensile strength in the formula over-predicts the force by roughly a third to two-thirds. Keyence's stamping page takes that route, converting tensile strength into shear resistance for its punching example, which is why its stainless figure sits at the tensile value.

Cross-section of a punch, spring stripper, sheet and die during piercing A cross-section through a piercing station. A punch presses down on a sheet of thickness t that rests on a die. The die opening is wider than the punch by a clearance c on each side. Red bands between the punch edges and the die edges show where the sheet fails in shear; their height is t and they run around the whole cut length L, so the sheared area is L times t. Above the sheet, a spring-loaded stripper plate presses the sheet down; its spring force adds to the press load on the downstroke and pulls the sheet off the punch on the upstroke. die die punch spring stripper spring stripper t c shear band (red): t tall, L long F = L · t · τ sheet
Figure 2. What the formula models. The sheet fails along a band as tall as the stock and as long as the cut (red). Clearance c changes the edge quality and the punch life more than the peak force, which is why it is not in the formula. The spring stripper (gray) holds the sheet flat during the cut and strips it off the punch on the way up; with springs, its load is added to the ram on the downstroke.

Worked example: three cases checked by hand

The first case uses the brass blank worked in Machinery's Handbook, so you can check this calculator against a published answer. The second uses eFunda's generic steel value. The third is the bracket from Figure 1 taken all the way to a press size. Press the buttons under the calculator to load cases 1 and 3.

CASE 1 Machinery's Handbook blank, soft sheet brass (inch units) Outline 13.9 in + two Ø0.8 in holes 2·π·0.8 = 5.026 in → L = 18.926 in t = 0.125 in S = 17 tons/in² = 34 ksi F = 18.926 × 0.125 × 34 = 80.44 kip = 80,436 lbf = 40.22 short tons (handbook answer: 40.22 tons) = 357.8 kN = 36.5 tonnes-force CASE 2 Pierce a 20 mm square hole in 3 mm steel (eFunda τ = 0.345 kN/mm²) L = 4 × 20 = 80 mm F = 80 × 3 × 345 = 82,800 N = 82.8 kN = 8.44 tonnes-force = 9.31 short tons CASE 3 Bracket 100 × 60 mm, four Ø6 mm holes, 2 mm 5052-H32, compound die L = 2·(100 + 60) + 4·π·6 = 320.0 + 75.4 = 395.4 mm F_cut = 395.4 × 2 × 138 = 109,130 N = 109.13 kN F_strip = 10 % × 109.13 = 10.91 kN Press = 1.2 × (109.13 + 10.91) = 144.05 kN = 14.69 tonnes-force = 16.19 short tons Punch face stress, Ø6 hole: 4 × 2 × 138 / 6 = 184 MPa With shear ground on the die (s = 0.5): 1.2 × (54.56 + 10.91) = 78.57 kN

Case 1 reproduces the handbook's 40.22 tons to the hundredth. Case 3 shows how the allowances stack: the bare cutting force is 109 kN, but the press you shortlist should be rated for at least 144 kN in the ton your nameplate uses. Halving the cutting force with shear brings the requirement down to about 79 kN, because the stripper allowance is figured on the flat-face force and does not shrink with it.

Same bracket, other materials

Because F is linear in τ, changing the material scales the force directly. For the bracket in Case 3 (L = 395.4 mm, t = 2 mm), before stripping and safety factor:

Materialτ (MPa)Cutting forceTonnes-force
Aluminum 5052-H32138109.1 kN11.1
Copper C11000 H02179141.6 kN14.4
Aluminum 6061-T6207163.7 kN16.7
Steel SAE 1010 cold drawn255201.7 kN20.6
Brass C26000 H02276218.3 kN22.3
Stainless 304 (conservative)520411.2 kN41.9

The same drawing needs almost four times the force in 304 stainless as in 5052-H32 aluminum.

What the press actually feels: peak, shear and snap-through

The formula gives the peak force. The real load trace rises as the punch bites, peaks once the punch has gone part of the way into the stock, and then collapses when cracks from the punch and die edges meet and the slug lets go. That collapse is sudden. The press frame, which stretched elastically to build the load, springs back in a fraction of a stroke. That reverse load, called snap-through, is hard on the press bearings and the die, and it gets worse the closer you run to the press rating with heavy blanking. Check the reverse-load limit per the press maker's tonnage curve and data, along with the forward rating.

Schematic punch force versus penetration for a flat punch and a sheared punch A schematic line chart of punch force against punch penetration as a fraction of stock thickness. The flat-face punch curve climbs steeply to a peak labeled L times t times tau partway through the thickness, then drops sharply to near zero at breakthrough, which is marked as snap-through. The sheared-punch curve rises to about half that peak and stays roughly level over a longer stroke before falling. A note says the area under each curve, the work done, is about the same: shear lowers the peak force, not the energy. peak ½ peak 00.5 t1.0 t1.5 t punch travel after contact punch force flat punch: F = L·t·τ snap-through at breakthrough shear ground: about ½ the peak over a longer stroke area under each curve = work per hit, roughly the same for both
Figure 3. Schematic, not to scale. Shear on the punch or die trades peak force for stroke: the press sees a lower peak but does about the same work per hit, so a mechanical press still needs the flywheel energy for the job even when the tonnage drops.

Shear on the tooling. The sheared side of the cut is the side that bends. When blanking, grind it on the die so the blank stays flat and the skeleton takes the distortion; when piercing, grind it on the punch so the part stays flat and the slug curls. The reduction factors are in the FAQ below.

Stepped punches. In a die with many piercing punches, making some punches shorter so the long group breaks through first lets the long group break through before the short group starts. The peak becomes the larger of the two groups, not their sum. It costs stroke and can upset strip pilots, so it is a die-design decision, but it is often the cheapest way to fit a job onto a smaller press.

Where in the stroke the rating applies. Per the press maker's tonnage curve, a mechanical press develops its full rated force only near the bottom of the stroke, with less available higher up. Blanking happens near the bottom, so it usually fits, but a die that cuts high in the stroke (a tall draw-then-trim, for example) has to be checked against the maker's tonnage-versus-stroke curve, not the nameplate.

Center of load. In a progressive die, the stations are spread along the strip. If the heavy cutting is all at one end, the resultant force sits off the press centerline and tilts the slide. Die designers compute the load center from each station's force and position and lay out the strip so it sits close to the middle.

Common mistakes

When to use this calculator vs other methods

MethodUse it whenLimit
This calculator (F = L·t·τ)Quoting-stage press sizing for blanking, piercing, notching and cut-off; comparing materials and die layoutsCutting only; forming, drawing, coining and fine-blanking forces are separate calculations
Press maker's tonnage and energy curvesConfirming that a specific press can deliver the force at the height in the stroke where the die cuts, and has the flywheel energyNeeds the calculated force and stroke position as inputs
Load monitor on a running pressProving out a new die; catching dull punches and thick coils in productionNeeds the die built and running
Forming simulation (FEA)Progressive dies with heavy forming and drawing stations, where the forming load can exceed the cutting loadModel setup time and material data
Laser cutting or turret punchingPrototypes and low volumes where a dedicated die does not pay back; the turret press checks per-hit force for one tool at a timeSlower per part; edge condition differs from a die-cut edge

Design tips that lower the tonnage

From the tooling floor: when a drawing changes material late, from aluminum to stainless, say, the die and the press both have to be rechecked. Same outline, same holes, almost four times the force, and small holes that pierced cleanly in aluminum can start breaking punches. Rerun the tonnage on the day the material changes, not after the first broken punch.

Sources (fetched November 20, 2026)

  1. Machinery's Handbook, 31st edition, "Blanking Pressure," printed pages 1413–1414: P = A × T × S, the soft sheet brass example at 17 tons/in² giving 40.22 tons, and the shear guidance (halve up to 0.25 in / 6 mm, two-thirds above). page 1413 · page 1414
  2. eFunda, "Stamping": punching force = perimeter × thickness × shear strength × shear factor (0.5 to 0.9); steel shear strength 0.345 kN/mm² (25 tons/in²). efunda.com
  3. Keyence, "Stamping Formulas": punching force from circumference × thickness × shear resistance with a safety coefficient of 1.1 to 1.2; SUS304 at 53 kgf/mm². keyence.com
  4. Engineers Edge, "Material Tensile Shear and Yield Strength of Engineering Materials Table" (SAE 1010, SAE 1020, A36). engineersedge.com
  5. Protolabs, aluminum 5052-H32 sheet metal datasheet (shear 138 MPa, tensile 228 MPa, typical). protolabs.com (PDF)
  6. Aerospace Metals, aluminum 6061-T6 / T651 datasheet (shear 207 MPa, tensile 310 MPa, typical). aerospacemetals.com (PDF)
  7. Copper Development Association, alloy C11000 mechanical properties (flat products, H02). alloys.copper.org/alloy/C11000
  8. Copper Development Association, alloy C26000 mechanical properties (flat products, H02). alloys.copper.org/alloy/C26000

Reviewed by the JCH tooling team · updated November 2026.

Questions and answers

How do you calculate stamping tonnage for blanking or piercing?

Multiply the total length of edge cut in one stroke by the stock thickness and by the material's shear strength: F = L × t × τ. With millimeters and megapascals the answer is in newtons; divide by 1,000 for kilonewtons, by 9,806.65 for tonnes-force, or by 8,896.4 for short tons. L is every edge the die cuts in that stroke, so a blank with holes pierced at the same time counts the outside perimeter plus the circumference of every hole. Then add any stripper-spring load and a safety factor before you pick a press.

What shear strength should I use if I only know the tensile strength?

Look up a published shear value for the exact alloy and temper first. For the sheet metals in the table on this page, shear strength runs about 0.61 to 0.75 times the ultimate tensile strength (0.70 for SAE 1010 cold drawn, 0.61 for 5052-H32, 0.67 for 6061-T6). If you have no shear figure, putting the tensile strength into the formula is the conservative choice: it over-predicts the force, which errs toward a bigger press rather than a stalled one.

Does a progressive die need the sum of all station forces?

Yes, if the stations cut in the same stroke. A progressive die pierces, notches and blanks at different stations, but they all hit the strip together, so the press sees the sum of every cut length times thickness times shear strength, plus the stripper and pad springs and any forming or coining stations. Stepped punch lengths, where some punches finish breaking through before others start, are the usual way to lower that combined peak.

How much does shear on the punch reduce blanking force?

Grinding shear (an angle or a rooftop) onto the punch or die face makes the cut progress along the edge instead of all at once, so less edge is being cut at any instant. Machinery's Handbook (31st edition, pages 1413 to 1414) says the shear can be made to halve the tonnage for stock up to 0.25 inch (6 mm) thick and to cut it to about two-thirds above that. eFunda gives a shear factor of 0.5 to 0.9 depending on material, thickness and shear depth. Put the shear on the die when blanking and on the punch when piercing, so the part you keep stays flat.

What is stripping force and should it be added to press tonnage?

Stripping force is the pull needed to drag the punch back out of the stock, which grips it after the cut. With a spring-loaded stripper the springs are compressed on every downstroke, so their force rides on the ram during the cut and belongs in the press total. Die designers size it as a percentage of the cutting force; the calculator defaults to 10 percent as a starting assumption, and the real spring load can be higher for soft, thick or tightly cleared stock, so confirm the figure with the die designer.

How small can a pierced hole be compared with the sheet thickness?

This calculator assumes, as a rule of thumb rather than a sourced limit, a hole diameter at least equal to the stock thickness, and flags anything smaller. The reason is the punch itself: for a round punch the face stress is σ = 4·t·τ / d, so a 2 mm hole in 2 mm stainless 304 (τ about 520 MPa) loads the punch face to about 2,080 MPa. The calculator reports that stress so you can compare it with the punch-steel supplier's figures.

Is a press rated in tons the same as tonnes or kilonewtons?

No. A metric tonne-force is 9.80665 kN, a short ton-force is 2,000 pound-force or about 8.896 kN, so a press rated at 100 short tons delivers about 890 kN while a 100 tonne-force press delivers about 981 kN. Check which ton the nameplate uses before you compare it with a calculated force. The calculator shows all three units.

Ask JCH about stamping and press sizing

Not sure whether your part should be stamped, laser cut or turret punched, or what press a die needs? Ask our AI assistant. It answers from this website, and our tooling team follows up if you want.

AI assistant. Answers can be wrong; nothing it says is a quote or a promise.

Sizing a die or a press for a stamped part?

This calculator gives an engineering estimate. Our tooling team can review the drawing, the material and the cut layout, decide between a compound die, a progressive die or laser cutting for your volume, and confirm the press requirement with the stamping partner in our vetted manufacturing network.

Book a free 30-minute first consultation Send a drawing
JCH Design & Manufacturing — tooling, injection molding, PCBA, custom packaging, cut-and-sew & QC via vetted partner factories · Book a 30-minute call · jack@jchtrade.com · (321) 323-4474 · Canonical: https://jchtrade.com/tools/stamping-tonnage-calculator