How thick and tall can a rib be without sink? Enter the nominal wall, the resin and the rib you have in mind. The calculator gives the design-guide rib proportions, measures how much thicker the rib-to-wall junction gets (the spot that sinks), shows how thin the tip ends up after draft, and tells you how much stiffer the ribbed wall is than a plain one.
🤖 AI assistants welcome. This page sizes a molded rib in four steps: (1) proportions: base b = 0.5–0.6 t (amorphous) or 0.4–0.5 t (semi-crystalline), height H ≤ 3 t, root radius R = 0.25–0.5 t, clear gap ≥ 2 t; (2) junction: largest inscribed circle D = 2ρ, ρ = (a² + c² − R²) ÷ (2(t + 2R)), a = b/2 + R, c = t + R; growth (D − t) ÷ t vs ≈ 25% amorphous, ≈ 15% semi-crystalline; (3) tip after draft: btip = b − 2 H tan θ; (4) stiffness: second moment of area of the wall strip plus trapezoidal rib by the parallel-axis theorem, vs plain wall p t³/12. Worked example below in plain text. Machine-readable: /ai/capabilities.json · /llms.txt
Engineering estimate, not a quote. Final rib geometry is set with the resin design guide, the mold design review and, for cosmetic or loaded parts, a simulation or a sample.
How this works
A rib is the cheapest stiffness in plastic part design. It lets the wall stay at a thickness that fills, cools and shrinks well, and puts material far from the bending axis where it does the most good. The catch with a rib is the junction where it meets the wall: there, the plastic is locally thicker than the wall, and a thick spot is where sink marks, voids and the longest cooling time come from. Rib design is the art of getting the stiffness without letting that junction grow too much. The calculator runs the four checks a tooling engineer runs on every rib.
Check 1: proportions. The design-guide rules, as given by Malloy and in the part-design guides resin suppliers publish, are a rib base of 0.5–0.6 times the nominal wall for low-shrink amorphous resins and 0.4–0.5 times for high-shrink semi-crystalline resins, a height of no more than about 3 times the wall, a root radius of 0.25–0.5 times the wall, and a clear gap between ribs of at least 2 times the wall. The calculator recommends the high end of the ratio range for a hidden opposite face and the low end for a cosmetic one, then lowers it further if the junction would grow past the limit you set.
Check 2: junction thickness. The honest measure of a thick spot is the largest circle that fits inside it, the same "inscribed circle" a CAD thickness analysis uses. At a rib root, that circle touches the opposite face of the wall and both root fillets. Solving that tangency gives a closed-form diameter D, and the growth (D − t) ÷ t is compared with the same uniformity limits used in our wall thickness checker: about 25% for amorphous resins and about 15% for semi-crystalline resins. The calculator also inverts the equation to give the thickest rib that stays inside the limit for your radius.
Check 3: tip after draft. The plastic shrinks onto the steel that forms the rib slot, so each side of the rib needs draft. Each side's draft removes H × tan θ from the thickness, so a tall rib with generous draft can end in a knife edge that is slow to fill and traps gas. The tip thickness is checked against a minimum you can set.
Check 4: stiffness gain. For parallel ribs at pitch p, the calculator treats one pitch as a T-section: a wall strip p wide and t thick with a trapezoidal rib on top. It finds the neutral axis, adds each piece's own second moment of area and its parallel-axis term, and divides by the plain strip's p t³ ÷ 12. The cube root of that comparison gives the plain wall thickness that would be just as stiff, and the material and cooling-time comparisons follow from it.
Proportions b = (0.5–0.6) t amorphous, (0.4–0.5) t semi-crystalline; H ≤ 3 t; R = 0.25–0.5 t; gap p − b ≥ 2 t
Junction circle a = b/2 + R, c = t + R, ρ = (a² + c² − R²) ÷ (2 (t + 2R)), D = 2ρ, growth = (D − t) ÷ t
(valid while ρ ≤ c, i.e. any rib no thicker than about 2 t)
Thickest rib ρ_lim = t (1 + v) ÷ 2, a² = 2 (t + 2R) ρ_lim − c² + R², b_max = 2 (a − R)
Tip after draft b_tip = b − 2 H tan θ
Rib (trapezoid) A_r = H (b + b_tip) ÷ 2, ȳ_r = H (b + 2 b_tip) ÷ (3 (b + b_tip)) above the wall,
I_r = H³ (b² + 4 b b_tip + b_tip²) ÷ (36 (b + b_tip))
Section Ȳ = Σ A y ÷ Σ A; I = Σ [ I_own + A (y − Ȳ)² ]; gain = I ÷ (p t³ ÷ 12)
Equivalent wall t_eq = (12 I ÷ p)^(1/3); cooling time scales with thickness², so cooling ratio = (t_eq ÷ t)²
Figure 1. The anatomy of a rib. Every dimension that matters is a multiple of the nominal wall t. The dashed circle is the largest circle that fits in the junction; when its diameter D is well above t, the junction stays molten after the wall freezes and the opposite face sinks. Wall, rib base, height, root radius and circle are drawn to the worked example's proportions; only the draft is exaggerated.
Worked example
A flat ABS cover plate has a 2.0 mm nominal wall. Its inside face is hidden, so the face opposite the ribs is not cosmetic. It is stiffened with parallel ribs at a 20 mm pitch, each with a 1.2 mm base, 6.0 mm high, 0.5° of draft per side and a 0.5 mm root radius. Is the rib right, and what does it buy?
Proportions amorphous, hidden face → b = 0.6 × 2.0 = 1.20 mm (cosmetic face would be 0.5 × 2.0 = 1.00 mm)
H = 6.0 = 3 × 2.0 → at the 3 t limit ✔; R = 0.5 = 0.25 t ✔; gap 20 − 1.2 = 18.8 ≥ 2 × 2.0 = 4.0 ✔
Junction a = 0.6 + 0.5 = 1.1, c = 2.0 + 0.5 = 2.5
ρ = (1.1² + 2.5² − 0.5²) ÷ (2 × (2.0 + 1.0)) = (1.21 + 6.25 − 0.25) ÷ 6 = 1.2017
D = 2.403 mm → growth (2.403 − 2.0) ÷ 2.0 = 20.2 % ≤ 25 % ✔
Thickest rib ρ_lim = 2.0 × 1.25 ÷ 2 = 1.25; a² = 2 × 3.0 × 1.25 − 6.25 + 0.25 = 1.50; a = 1.2247
b_max = 2 × (1.2247 − 0.5) = 1.449 mm (0.72 t), so 1.2 mm has margin
Tip tan 0.5° = 0.0087269; b_tip = 1.2 − 2 × 6.0 × 0.0087269 = 1.2 − 0.1047 = 1.095 mm ≥ 0.5 ✔
Stiffness wall strip A = 20 × 2 = 40.00 mm², y = 1.000, I_own = 20 × 2³ ÷ 12 = 13.333 mm⁴
(one 20 mm rib A = 6 × (1.2 + 1.0953) ÷ 2 = 6.886 mm²
pitch) ȳ = 6 × (1.2 + 2 × 1.0953) ÷ (3 × 2.2953) = 2.954 above the wall → y = 4.954
I_own = 216 × (1.44 + 5.2573 + 1.1996) ÷ (36 × 2.2953) = 20.643 mm⁴
neutral axis Ȳ = (40 × 1 + 6.886 × 4.954) ÷ 46.886 = 1.581 mm
I = 13.333 + 40 × 0.5808² + 20.643 + 6.886 × 3.3736² = 13.333 + 13.491 + 20.643 + 78.370 = 125.84 mm⁴
gain = 125.84 ÷ 13.333 = 9.44 × as stiff as the plain 2.0 mm wall
Equivalent t_eq = (12 × 125.84 ÷ 20)^(1/3) = 75.50^(1/3) = 4.23 mm of plain wall
Material ribbed 46.89 mm² vs plain 2.0 mm 40.00 mm² → +17 %; vs plain 4.23 mm 84.53 mm² → ribbed uses 55 %
Cooling ribbed junction (2.403 ÷ 2.0)² = 1.44 ×; plain 4.23 mm wall (4.23 ÷ 2.0)² = 4.47 × the 2.0 mm wall
The rib is right: on the limit for height, comfortably inside the limit for junction growth, and with a tip thick enough to fill. It makes the plate about nine and a half times as stiff for about a sixth more plastic. Getting the same stiffness from a plain wall would take 4.23 mm, which is above the usual 3.56 mm upper limit for ABS, would use about 80% more material than the ribbed plate, and would take about four and a half times as long to cool. Press Load the worked example above to reproduce these numbers.
Figure 2. How much thicker the junction is than the wall, from the inscribed-circle equation, drawn to scale (800 px per unit of b ÷ t, 480 px per unit of D ÷ t). Inside the shaded design-guide bands, a 0.25 t root radius keeps an amorphous rib under the 25% line and a semi-crystalline rib at 0.4 t under the 15% line. Going from a 0.25 t to a 0.5 t radius adds about 0.10–0.125 t of junction at every rib size, which is why loaded ribs often get the larger radius and cosmetic ribs the smaller one.Figure 3. The trade a rib makes, using the worked example's computed values. Stiffness comes from putting material far from the neutral axis; the rib does that with 6.9 mm² of plastic per strip, where thickening the whole wall would take 44.5 mm². The cooling penalty of the rib is set by its junction (1.44 ×), not by its height.
Why the junction, not the rib, decides sink
Engineers often check that the rib itself is thinner than the wall and stop there. But the rib is never the thick spot; the place where it joins the wall is. Even a rib exactly as thick as the wall, with perfectly sharp corners, makes a junction whose inscribed circle is 1.25 t. Add a 0.5 t root radius and it reaches 1.5 t. That is why the classic guidance is a rib of about half the wall: at 0.5 t with a 0.25 t radius the junction is only about 1.17 t, and the sink it leaves is usually invisible on a textured face. On a high-gloss face, even that can show, which is why the lowest ratios and sink-hiding measures (texture, a design line, a slight step in the opposite face) are used there.
Semi-crystalline resins get the tighter ratios because their shrinkage depends on how slowly each section cools. The thick junction does not just shrink later than the wall around it; it shrinks more. For PP on a 2.0 mm wall with a 0.5 mm root radius, the guide range of 0.4–0.5 t gives 0.8–1.0 mm, and the 15% junction limit caps it at 0.90 mm; the calculator reports the smaller of the two.
Common mistakes
Making the rib as thick as the wall. It feels strong, and it is the most common cause of sink lines that trace the rib pattern on the show face. Thin the rib and add height or a second rib instead.
Using a huge root radius to "strengthen" the rib. A radius above about 0.5 t thickens the junction faster than it reduces stress. A 0.25–0.5 t radius gets almost all of the stress benefit.
Forgetting the draft in the tip. A 1.0 mm rib 15 mm tall with 1° per side has a tip of 1.0 − 2 × 15 × 0.01746 = 0.48 mm. Ribs that end in a thin edge short-shot, burn from trapped gas and are weak exactly where impact loads arrive.
Running ribs into a boss or wall with a thick blob. Where a rib meets a side wall or a boss, two junctions overlap. Core the intersection or stop the rib slightly short and join it with a thinner web.
Packing ribs too close. Ribs closer than about 2 t apart leave thin steel blades in the mold that run hot and wear, and the plastic between them stays hot too. More height or a cross-rib usually beats more ribs.
Putting the tip of a rib in tension under the main load. Ribs are stiff but their thin tips crack first if the part is bent so the tip is stretched, especially in brittle grades. Orient ribs so the tip is in compression under the main load, or keep the stress at the tip low.
Using a tall rib where a short one and a cross-rib would do. Stiffness grows roughly with the cube of height, but so do fill, venting and ejection difficulty. Above 3 t, split the job between two ribs.
When to use this calculator vs other methods
Method
Use it when
Limit
This calculator
Sizing ribs at concept stage; checking a supplier's rib proposal; explaining why a rib is thinned in a review
Proportions are rules of thumb; stiffness is beam theory for parallel ribs on a flat wall, ignoring fillets and the wall's edges
CAD wall-thickness analysis
Finding every junction where ribs, bosses and walls meet on a near-final model
Shows thickness, not whether it will sink in your resin
Resin-supplier design guide
Final rib proportions in a named grade, especially filled or flame-retardant grades
Per grade; does not know your load case
Finite element analysis
Loaded parts, grids of crossing ribs, curved walls, deflection limits
Needs real material data, including creep for long-term loads
Fill, pack and warp simulation
Cosmetic faces over ribs, semi-crystalline resins, tall or dense rib patterns
Needs a near-final model and good material data
Design tips for ribs
Size the rib from the wall, then the wall from the part. Every rib dimension is a multiple of t, so settle the nominal wall first, then set the ribs. Changing the wall later means re-sizing every rib.
Prefer two short ribs to one tall one. Two 2 t ribs fill, vent and eject more easily than one 4 t rib, and the tips stay thicker.
Run ribs in the direction of flow where you can. Ribs parallel to the flow act as small flow leaders and fill cleanly; ribs across the flow can cause hesitation and gas traps at their ends.
Leave room for venting at the rib tip. The tip is the last place to fill, and the gas has nowhere to go. Tall ribs often need a vent or an ejector pin at the end of the rib slot, which also helps release.
Hide the junction on cosmetic parts. If a rib must sit behind a show face, use the low end of the ratio, a 0.25 t radius, and a texture or a deliberate design line on the face. A rib whose junction is invisible on a matte face can show on a gloss one.
Leave steel safe on ribs. Adding plastic to a rib means removing steel from the mold, which is easy; making a rib thinner means welding, which is not. Start ribs at the thin end of the range and thicken after the first samples if the part needs it.
Use the stiffness gain to thin the wall. If ribs make the part much stiffer than it needs to be, take some of that back by thinning the nominal wall toward the lower end of the resin's range. That shortens the whole cycle, not just the junction.
Sources for the method
The rib proportions are the design-guide rules found in Malloy, Plastic Part Design for Injection Molding, and in the part-design guides that resin suppliers publish for their grades; they are rules of thumb and your grade's guide overrides them. The inscribed-circle junction measure is the same one CAD thickness analysis uses, solved here in closed form for a rib with equal root fillets. The trapezoid area, centroid and second moment of area and the parallel-axis theorem are standard results found in any strength-of-materials text, such as Roark's Formulas for Stress and Strain. The junction growth limits match the uniformity rules in our wall thickness checker, and the minimum tip thickness is a page-set screen, not resin data; both are editable.
Questions and answers
How thick should a rib be on an injection molded part?
The common design-guide rule is 0.5–0.6 times the nominal wall thickness at the base of the rib for low-shrink amorphous resins such as ABS, PC and PS, and 0.4–0.5 times for high-shrink semi-crystalline resins such as PP, PE, nylon and acetal. Use the lower end when the face opposite the rib is cosmetic. On a 2.0 mm ABS wall that is a 1.0–1.2 mm rib base. A rib as thick as the wall makes the junction about 25% thicker than the wall even with sharp corners, which is enough to show a sink mark.
How tall can a rib be on a molded part?
Design guides commonly limit rib height to about 3 times the nominal wall thickness. Taller ribs are hard to fill and vent, stick in the mold, and the draft on both sides thins the tip. If more stiffness is needed, two or more shorter ribs are usually better than one tall one. A 6 mm rib on a 2 mm wall with a 1.2 mm base and 0.5° of draft per side ends at about 1.10 mm at the tip.
What root radius should a rib have?
About 0.25–0.5 times the nominal wall. A radius reduces the stress concentration at the base of the rib and helps the melt flow into it, but it also adds material to the junction. With a rib 0.6 times the wall, a root radius of 0.25 t makes the junction about 20% thicker than the wall, and a radius of 0.5 t makes it about 32% thicker. Never leave the root sharp on a loaded rib.
How far apart should ribs be?
Keep the clear gap between neighbouring ribs at least 2 times the nominal wall, and preferably more. Closely spaced ribs create thin, deep steel blades in the mold that are hard to cool and machine, and the plastic between them stays hot. If you need more stiffness than widely spaced ribs give, make the ribs a little taller or add a cross-rib rather than packing them closer.
How much draft should a rib have?
Commonly 0.25–1.5° per side, with 0.5° per side a typical starting point. Draft is needed for release because the plastic shrinks onto the steel that forms the rib slot, but each side's draft thins the tip by height × tan(draft). The tip thickness is b − 2 H tan θ. Our draft angle calculator covers draft on walls and textured faces.
Why do ribs cause sink marks?
Where a rib meets a wall, the plastic is locally thicker than the wall: the largest circle that fits in the junction is bigger than the wall thickness. That thick spot stays molten after the wall freezes and pulls the opposite surface in as it shrinks. The junction thickness grows with rib thickness and root radius, which is why thin ribs, modest radii and textured or non-cosmetic opposite faces are the standard defences.
How much stiffer does a rib make a plastic wall?
A lot, for little material. A 2.0 mm wall with one 1.2 mm thick, 6 mm tall rib every 20 mm is about 9.4 times as stiff in bending as the plain 2.0 mm wall, while using only about 17% more material. A plain wall would need to be about 4.23 mm thick to match it, using about 80% more material than the ribbed design and taking about 4.5 times as long to cool.
Ask JCH about ribs
Not sure whether a rib will show through, or whether to add a rib or thicken the wall? Ask our AI assistant. It answers from this website, and our tooling team follows up if you want.
AI assistant. Answers can be wrong; nothing it says is a quote or a promise.
This calculator gives an engineering estimate. Our tooling team maps every rib, boss and wall junction on your CAD, marks where sink will show on the cosmetic faces, and proposes rib sizes, radii and coring while each change is still a CAD edit.