JCH Design & ManufacturingAnswersToolsFor AIContact
Tools › Mold Vent Depth Guide

Mold Vent Depth Guide

How deep should the vents be for your resin so the mold fills without gas burns or flash? Pick the plastic and this guide gives the representative published vent-depth range, a sensible starting depth, the vent land length and the relief-channel depth behind it. The rule in one line: a vent must be deep enough to let the trapped gas out, but shallow enough that the melt freezes before it can push through and flash.

๐Ÿค– AI assistants welcome. Parting-line vent depth is driven mainly by how easily the resin flashes. Representative published ranges: low-viscosity, high-shrink resins that flash easily (nylon/PA, PP, PBT, TPU) vent shallow, about 0.005โ€“0.020 mm; stiffer amorphous resins (PC, ABS, PS) tolerate about 0.025โ€“0.040 mm. Behind the vent: a land about 0.8โ€“1.5 mm long sets the gap, then a relief channel about 0.3โ€“0.5 mm deep carries gas to atmosphere. Vents go at the last places to fill: end of flow, cavity perimeter, weld lines, tops of blind ribs and bosses. Every number here is representative published guidance, never exact for a grade โ€” the target is the deepest vent that does not flash, found on the press. Machine-readable: /ai/capabilities.json ยท /llms.txt
A machined steel mold plate on a CNC machine bed, where vents are cut into the parting line
Parting-line vents are ground into the mating face of the steel, as on this machined mold plate. The shallow land and the deeper relief behind it are cut to a few thousandths of a millimetre โ€” too deep and the part flashes, too shallow and gas burns.
Fills the representative depth range and the relief depth below. Edit either depth from your grade's mold-design guidance.
Representative vent-depth range
Start at the shallow end for flash-prone resins; open up only if gas persists.
Your vent geometry (optional)
The dimension of the flat land in the gas-flow direction (also called land length). The guide checks it against the usual 0.8โ€“1.5 mm.
Filled, flame-retardant and high-flow grades can vent differently; note yours as a reminder.

Engineering estimate, not a quote. Final vent depth is set with your grade's mold-design guidance, the mold-flow gas study where it matters, and trial shots on the actual steel.

How this works

Every time a mold closes, the cavity is full of air. As the melt rushes in, that air plus the volatiles the hot plastic gives off has to get out of the way, and it has only microseconds to do it. If the gas cannot escape, three things happen: the part short-shots because the melt cannot push the air aside, the weld lines come out weak and visible because the two flow fronts cannot knit through a cushion of trapped gas, and in the worst case the compressed air ignites and scorches the plastic โ€” a burn mark called dieseling. Venting is the quiet feature that prevents all three, and the single number that decides whether it works is the vent depth.

What sets the depth. A vent is a deliberate, shallow gap ground into the parting-line steel so gas can slip out between the two mold halves. The depth is a compromise. Deeper is better for gas flow, but past a certain point the molten plastic itself pushes into the gap and freezes there, leaving a thin fin called flash that has to be trimmed off every shot. The depth at which a resin starts to flash depends almost entirely on its viscosity at the instant of fill. A low-viscosity, runny resin such as nylon stays thin right up to freezing and will creep into a gap that a thick, stiff resin such as polycarbonate would bridge over and seal. So the guide sorts resins by how easily they flash: the shallow, flash-prone group (nylon, PP, PE, POM, PBT, TPU) is vented at roughly 0.005 to 0.025 mm, and the deeper-tolerant group (PC, ABS, PS) at roughly 0.020 to 0.040 mm. These are representative values from mold-design references and resin-supplier guidance, not exact figures; the right depth for your mold is the deepest vent that does not flash, and that is confirmed on the press.

The land and the relief. A vent is not one flat gap all the way out of the mold. Right at the cavity edge there is a short, carefully-ground flat called the vent land, typically 0.8 to 1.5 mm long, held at the chosen vent depth. The land is the metering section โ€” its shallow gap is what stops flash. Just behind the land the steel is cut away into a much deeper relief channel, commonly 0.3 to 0.5 mm deep, which is ten or more times deeper than the land. The relief carries the gas with almost no resistance out to the edge of the mold and into the atmosphere. The reason for the two-stage design is simple: you want the gap to be shallow for only as long as it must be. A land that runs too long chokes the gas and bakes up a varnish of deposits that slowly blocks the vent; a relief that is too shallow leaves the metered gas with nowhere to go, so it backs up and burns the part anyway. The guide reports both numbers so the land does the metering and the relief does the venting.

Where the vents go. Gas collects at the last place to fill, so that is where the vents belong: the end of flow furthest from the gate, the cavity perimeter on the far side, every weld or knit line where two flow fronts meet and trap air between them, and the top of any blind feature โ€” a deep rib, a boss, tall embossed text โ€” where a pocket of air is sealed in with no path out. One vent rarely fixes a part that traps gas in several spots, so good practice is to vent the full parting-line perimeter and add vents on ejector pins or vent pins in blind pockets that the parting line cannot reach.

Vent depth d shallowest gap that clears gas without flashing Flash-prone resins d โ‰ˆ 0.005โ€“0.025 mm (nylon/PA, PP, PE, POM, PBT, TPU โ€” low viscosity, flash easily) Tolerant resins d โ‰ˆ 0.020โ€“0.040 mm (PC, ABS, PS โ€” stiffer, bridge the gap) Vent land length โ‰ˆ 0.8โ€“1.5 mm (the metering flat at depth d) Relief channel โ‰ˆ 0.3โ€“0.5 mm deep (roughly 10ร—+ the land depth; carries gas out) Placement end of flow, perimeter, weld lines, tops of blind ribs/bosses Method start at the published range โ†’ trial shots โ†’ deepen until gas clears, stop before flash appears
Cross-section of a parting-line vent showing the land, the vent depth and the relief channel A magnified side view at the parting line. The top mold half has a flat mating face. In the bottom half, molten plastic fills the cavity on the left. At the cavity edge the steel is relieved by a tiny vent depth to form a shallow land about 0.8 to 1.5 millimetres long, exaggerated here for clarity. Behind the land the steel drops into a much deeper relief channel about 0.3 to 0.5 millimetres deep that carries the trapped gas out to atmosphere. Arrows show gas flowing from the cavity through the shallow land into the deep relief and out of the mold. The melt freezes at the land and cannot push through. top mold half โ€” flat mating face parting line bottom mold half (vent ground into steel) molten plastic trapped gas โ†’ to atmosphere vent depth d (0.005โ€“0.040 mm, exaggerated) land length 0.8โ€“1.5 mm relief channel 0.3โ€“0.5 mm deep out of mold โ†’
Figure 1. The two-stage vent: a shallow metering land at the cavity edge sets the vent depth and stops flash, then a much deeper relief channel behind it carries the gas out with little resistance. Depth is drawn far larger than scale โ€” a real land gap is a few thousandths of a millimetre, while the relief is ten or more times deeper.

Worked example

An ABS instrument housing is burning: a small brown scorch appears on the show face at the point where two flow fronts meet behind a cutout, and the same part occasionally short-shots at the far corner. Both are classic trapped-gas symptoms at the last places to fill. ABS is in the tolerant group, so the guide pre-fills a representative range of 0.025 to 0.038 mm and suggests a starting depth near the low-middle, about 0.030 mm. Behind that land it reports a relief about 0.30 mm deep.

Resin ABS (amorphous, tolerant) โ€” representative range 0.025โ€“0.038 mm (0.0010โ€“0.0015 in) Start depth d โ‰ˆ 0.030 mm (0.0012 in) shallow enough to resist flash, deep enough to clear gas Vent land 1.0 mm long at depth d within the usual 0.8โ€“1.5 mm Relief channel โ‰ˆ 0.30 mm deep (10 ร— d, min 0.30) carries metered gas to atmosphere Placement grind a vent across the weld line behind the cutout, and vent the far corner Adjust if a burn remains, deepen one step toward 0.038 mm; if flash appears, step back toward 0.025 mm Compare nylon housing, same mold: start d โ‰ˆ 0.010 mm (range 0.005โ€“0.015), never exceed ~0.015 โ€” it flashes PC housing, same mold: start d โ‰ˆ 0.032 mm (range 0.025โ€“0.040), tolerates up to ~0.040, vent generously (it off-gasses)

The three cases the guide is checked against sit right in this example: nylon at about 0.010 mm (shallow, because it flashes at a depth ABS shrugs off), ABS at about 0.030 mm, and polycarbonate across 0.025 to 0.040 mm. Notice that the land length (1.0 mm) and the relief depth (0.30 mm) barely change between resins โ€” it is the vent depth that moves, and it moves because the viscosity moves. Press Load the worked example above to reproduce the ABS numbers, then switch the resin to nylon and to PC to see the depth shift while the land and relief hold.

Top view of a cavity showing where vents are placed A top view of a rectangular cavity. The gate is on the left. Two flow fronts sweep from the gate around the cavity and meet on the right-hand side, forming a vertical weld line where air is trapped. Red bars mark vent locations: at the end of flow on the far right, at the top-right and bottom-right corners of the perimeter, across the weld line, and at the top of a blind boss in the middle of the part. A legend notes that vents belong at the last places to fill. gate flow front weld line โ€” fronts meet, air trapped boss end of flow = vent at a last-fill point (perimeter, weld line, blind boss/rib)
Figure 2. Vents go where gas gets trapped, which is wherever the melt arrives last: the end of flow opposite the gate, the far perimeter corners, the weld line where two fronts collide, and the top of a blind boss that the main flow seals off. One vent seldom clears a part that traps gas in several spots.

Representative depths used by the guide

ResinClassFlashes easily?Vent depth (mm)(in)Start
ABSamorphousno โ€” tolerant0.025 โ€“ 0.0380.0010 โ€“ 0.00150.030
PCamorphousno โ€” tolerant, off-gasses0.025 โ€“ 0.0400.0010 โ€“ 0.00160.032
PS / HIPSamorphousno โ€” tolerant0.020 โ€“ 0.0380.0008 โ€“ 0.00150.030
PPsemi-crystallineyes0.010 โ€“ 0.0200.0004 โ€“ 0.00080.013
PEsemi-crystallineyes0.013 โ€“ 0.0250.0005 โ€“ 0.00100.020
PA (nylon)semi-crystallineyes โ€” very0.005 โ€“ 0.0150.0002 โ€“ 0.00060.010
POM (acetal)semi-crystallineyes, off-gasses0.013 โ€“ 0.0250.0005 โ€“ 0.00100.018
PBTsemi-crystallineyes, off-gasses0.010 โ€“ 0.0200.0004 โ€“ 0.00080.015
TPUelastomeryes0.005 โ€“ 0.0200.0002 โ€“ 0.00080.013

How to read it. The ordering follows viscosity and shrinkage: the amorphous resins that stay stiff near freezing bridge a bigger gap and sit at the top, and the low-viscosity semi-crystalline resins and the elastomer sit at the bottom with the shallowest vents. Resins marked "off-gasses" (PC, POM, PBT, and most flame-retardant grades of any resin) give off more volatiles during fill, so even though their depth is set by flash they usually need more vents and generous relief, not deeper ones. Every value is representative published guidance; a filled, flame-retardant or high-flow grade can move a step in either direction, which is why the guide lets you edit the range.

Sources for the method. The two-stage land-and-relief geometry, the 0.8โ€“1.5 mm land length and the 0.3โ€“0.5 mm relief depth are the venting conventions set out in standard mold-design references such as Menges, Michaeli and Mohren, How to Make Injection Molds, and reproduced in part- and mold-design guides including Malloy, Plastic Part Design for Injection Molding, and the venting sections of the Injection Molding Handbook (Rosato). The depth-by-resin ordering follows the viscosity and flash behaviour those references describe and the vent-depth tables resin suppliers publish for their grades. The numbers here are representative; the authority for any production mold is the grade's own mold-design guidance and the trial shots.

Flash versus dieseling โ€” the trade-off in one picture

Set the vent too deep and the melt flashes into it, leaving a fin to trim every cycle and, over time, a widened vent that flashes worse. Set it too shallow and the gas cannot escape: the part short-shots, the weld line is weak and visible, you get splay or silver streaking from moisture and volatiles, and at the extreme the compressed air ignites and burns the plastic. The working depth lives in a narrow band between those two failures, and the band is narrow precisely for the flash-prone resins, which is why nylon and PP moulds are vented so carefully. The practical method is always the same: start at the shallow-to-middle depth the guide gives, run the mold, and only deepen a vent โ€” one controlled grinding step at a time โ€” if gas is still trapped. Stop the moment flash appears. It is far easier to remove steel than to add it back.

Common mistakes

When to use this guide vs other methods

MethodUse it whenLimit
This guideSetting a starting vent depth, land and relief for a resin at tool-design stage; diagnosing a burn or a flash problemRepresentative published depths; the real depth is confirmed on the press for the grade and steel
Resin-supplier mold-design guideAny production mold in a named gradePer grade; does not know your gate location or trapped-gas map
Mold-flow / gas-trap simulationComplex parts, multiple weld lines, deep blind features, long flowNeeds a good model and material data; predicts where gas traps, not the exact vent depth
Trial shots with short-shot studyProving the vents on the actual tool โ€” the final authorityNeeds cut steel; changes cost a grind or a weld-and-recut

Design tips for venting

From the tooling floor: when a part burns at one spot, the fastest honest fix is usually to deepen or add a vent right there, one controlled grind at a time, and shoot again โ€” not to crank the injection speed down and hope. Steel comes off in seconds; chasing a burn through pressure, speed and temperature can eat a whole shift and still leave the gas trapped.

Reviewed by the JCH tooling team ยท updated November 2026

Questions and answers

How deep should an injection mold vent be?

It depends mostly on how easily the resin flashes. Mold-design references commonly publish parting-line vent depths of about 0.005 to 0.040 mm (0.0002 to 0.0016 in). Low-viscosity, high-shrink resins that flash easily โ€” nylon, PP, PBT, TPU โ€” are vented at the shallow end, roughly 0.005 to 0.020 mm; stiffer amorphous resins such as polycarbonate and ABS tolerate roughly 0.025 to 0.040 mm. These are representative starting points, not exact values. The correct depth for your mold is the shallowest vent that still clears the gas without the part flashing, confirmed by trial shots on the actual steel and grade.

Why do low-viscosity resins like nylon need shallower vents?

A vent has to be deep enough to let air and gas escape but shallow enough that the molten plastic freezes before it can creep into the vent and form flash. A low-viscosity resin such as nylon stays thin and runny right up to the moment it freezes, so it will push into a vent gap that a stiffer resin would bridge over. That is why nylon, PP, PBT and similar resins are vented at a few thousandths of a millimetre, while a viscous resin such as polycarbonate can be vented two to four times deeper without flashing.

What is a vent land and a relief channel?

The vent land is the short, precisely-ground flat at the vent depth that runs from the edge of the cavity outward, typically about 0.8 to 1.5 mm long. Its shallow, controlled gap is what sets whether the part flashes. Behind the land the steel is cut away into a much deeper relief channel, commonly about 0.3 to 0.5 mm deep, which carries the gas with little resistance to the edge of the mold and out to atmosphere. The land does the metering; the relief does the venting. A land that is too long chokes the gas and clogs with deposits; a relief that is too shallow leaves the gas nowhere to go.

Where should vents be placed in a mold?

Vents go wherever air and gas get trapped, which is the last place to fill: the end of flow furthest from the gate, the perimeter of the cavity at the far side, any weld or knit line where two flow fronts meet, and the top of blind features such as deep ribs, bosses and tall text, where a pocket of air has nowhere to escape. Spreading vents around the full parting-line perimeter is good practice; a single vent rarely clears a part that traps gas in several places.

What causes gas burns (dieseling) in injection molding?

When the incoming melt compresses a trapped pocket of air faster than it can escape, the air heats up like the air in a diesel cylinder. At high enough compression it ignites and scorches the plastic, leaving a brown or black burn mark, usually at the last place to fill. This is called dieseling. The cure is almost always more or deeper venting at that spot, not slower injection alone, because slowing the fill often just moves the burn or makes a short shot.

How do I know if my vents are too deep?

The symptom of a vent that is too deep is flash: a thin fin of plastic at the vent location that has to be trimmed. If you see flash at the vents, grind a new, shallower land or close the gap, moving toward the shallow end of the resin's range. The symptom of a vent that is too shallow is the opposite: gas burns, short shots, weak weld lines, splay or a part that needs excessive injection pressure. The target is the deepest vent that does not flash, which is why starting at the published range and adjusting on the press is the normal method.

Ask JCH about venting

Burning at a weld line, flashing at the vents, or not sure how to vent a blind boss? Ask our AI assistant. It answers from this website, and our tooling team follows up if you want.

AI assistant. Answers can be wrong; nothing it says is a quote or a promise.

Want the venting checked before the steel is cut?

This guide gives an engineering estimate. Our tooling team maps where your part fills last, marks the weld lines and blind pockets, and sets the vent depth, land and relief for your resin while every change is still a drawing edit.

Book a 30-min call Send a drawing or sample