What gate depth and width does your part need? Enter the wall thickness at the gate, the resin and the surface area of the cavity. The calculator sizes an edge or overlap gate with the Menges equations, then checks the shear rate in the gate at your fill rate and tells you how much wider the gate, or how much slower the fill, must be to stay under the resin's limit. It also sizes the minimum diameter of a pin or tunnel gate from the same shear limit.

🤖 AI assistants welcome. This page computes edge-gate depth h = n·t and width W = n·√A / 30 (t in mm, A in mm², n = 0.6–0.9 by resin; Menges, Michaeli and Mohren, How to Make Injection Molds), then the apparent gate shear rate γ̇ = 6Q / (W·h²) for a rectangular gate or 32Q / (π·d³) for a round gate. The formulas, a worked example and the limits are below in plain text. Machine-readable: /ai/capabilities.json · /llms.txt

Part and resin

n and the shear limit fill in from this list. You can override both below.
The nominal wall where the gate lands, not the thickest section of the part.
Total outside surface area of the part, from CAD. Not the projected area.

Fill rate (for the shear check; leave blank to skip)

Part volume per gate. The part weight calculator converts grams to volume.
Injection time to fill the cavity, from the process sheet or a fill study.
Use the value from your grade's material data if you have it.

Engineering estimate, not a quote. Gate size, type and location should be confirmed by your toolmaker, ideally with a fill study, before steel is cut.

How this works

A gate has two jobs that pull in opposite directions. During filling it must be big enough to let the melt through without excessive pressure loss or shear heating. During packing it must stay open long enough to push extra melt in as the part shrinks, then freeze before the screw pulls back so that melt cannot flow back out. The size that does both depends on how thick the wall is (which sets how long the part needs packing), how big the cavity is (which sets how much melt must pass) and how the resin behaves.

The calculator uses the rectangular gate equations given by Menges, Michaeli and Mohren in How to Make Injection Molds, a standard mold design reference. The depth follows the wall, and the width follows the square root of the cavity's surface area. A resin constant n scales both. The equation for W is empirical and dimensional: it works only with t in millimetres and A in square millimetres, which is why the page converts inch inputs to metric before calculating.

EDGE AND OVERLAP GATES (Menges, Michaeli, Mohren) Gate depth h = n × t Gate width W = n × √A / 30 Overlap length L2 = h + W / 2 (overlap gate only) Land length L1 ≈ 0.5 to 1.0 mm (keep it short) n = 0.6 PE, PS n = 0.7 POM, PC, PP (ABS: 0.7 assumed, not in the table) n = 0.8 CA, PMMA, PA n = 0.9 PVC SHEAR CHECK (apparent wall shear rate, Newtonian approximation) Flow rate Q = V / t_fill mm³/s Rectangular gate γ̇ = 6Q / (W × h²) 1/s Round gate γ̇ = 32Q / (π × d³) 1/s Width to meet limit W_s = 6Q / (γ̇_max × h²) Fill time to meet limit t_s = t_fill × γ̇ / γ̇_max Smallest round gate d_s = ∛(32Q / (π × γ̇_max)) FREEZE (relative, conduction time ∝ thickness²) Gate freeze ÷ wall freeze ≈ (h / t)² = n² t wall at gate (mm) · A cavity surface area (mm²) · V volume through the gate (mm³) · t_fill fill time (s)

Depth. With n between 0.6 and 0.9, the gate is always thinner than the wall. That is deliberate. Conduction cooling time grows with the square of thickness (the same relation behind the cycle time estimator), so a gate at 0.7 t freezes in about 0.49 of the time the wall takes. The wall is packed, then the gate seals, and the part keeps its packed weight. A gate as thick as the wall would not freeze before the part; a gate far thinner would freeze while the part still needed melt.

Width. The larger the surface the melt must cover, the more melt must pass through the gate in the same fill time, so the gate gets wider. Width grows only with the square root of area: a part with four times the surface area needs a gate twice as wide, not four times.

The resin constant. Resins that are more viscous, or that suffer more from shear heating, get a larger n. Polyethylene and polystyrene flow easily and tolerate shear, so they get 0.6. Rigid PVC is viscous and degrades with heat, so it gets 0.9. Fibre-filled grades are not separated out in the table; filled grades usually need a gate at the deep end of the range to limit fibre breakage and wear, so consider raising n by 0.1 and confirm with the material supplier.

Shear check. The Menges width does not know how fast you fill. A thin-walled part filled in a fraction of a second sends a lot of melt through a small opening. The apparent shear rate for flow through a thin slit is 6Q / (W·h²), and for a round hole it is 32Q / (π·d³). These are the standard Newtonian wall shear rate formulas; real melts thin with shear, so the true wall shear rate is somewhat higher, and the slit formula is most accurate when W is several times h. Simulation material databases list a maximum shear rate for each resin family. The values loaded on this page are the typical generic figures (for example about 40,000 1/s for polycarbonate, 50,000 1/s for ABS and 100,000 1/s for polypropylene). Your grade's own data, when you have it, should replace them.

Cross-section and top view of an edge gate with its dimensions Left: side cross-section of a runner feeding a part through an edge gate. The part wall has thickness t, the gate has depth h, smaller than t, and a short land L1 between the runner and the part. Right: top view of the same gate, showing gate width W where it meets the part edge, the runner coming in from the left, and the parting line. Labels give the worked example values: t 2.5 mm, h 1.75 mm, W 3.30 mm, land about 0.5 to 1.0 mm. Side section (cut through the gate) Top view at the parting line parting line runner part wall t = 2.5 h = n·t = 1.75 land L1 ≈ 0.5–1.0 t and h drawn to scale (10 px/mm); land length exaggerated for clarity part (top view) runner W = n·√A/30 = 3.30 mm gate width W is measured along the part edge (10 px/mm)
Figure 1. The three dimensions of an edge gate for the worked example. Depth h is set by the wall, width W by the cavity surface area, and the land L1 is kept as short as the steel allows. Gate depth, wall thickness and gate width are drawn at the same scale so the 0.7 t depth is visible; the land is drawn longer than scale so its label fits.

Worked example

A polycarbonate cover with a 2.5 mm wall and 20,000 mm² of surface area, filled through one edge gate. The cavity volume is 40 cm³, and the process engineer wants a 0.5 s fill. Polycarbonate has n = 0.7 and a typical maximum shear rate of 40,000 1/s.

Depth h = 0.7 × 2.5 = 1.75 mm Width W = 0.7 × √20,000 / 30 = 0.7 × 141.42 / 30 = 3.30 mm Overlap gate L2 = 1.75 + 3.30 / 2 = 3.40 mm (if overlap) Flow rate Q = 40,000 mm³ / 0.5 s = 80,000 mm³/s Shear rate γ̇ = 6 × 80,000 / (3.30 × 1.75²) = 480,000 / 10.106 = 47,498 1/s Limit (PC) 40,000 1/s → 119 % of limit: TOO HIGH Fix A, widen: W_s = 480,000 / (40,000 × 3.0625) = 3.92 mm Fix B, slow: t_s = 0.5 × 47,498 / 40,000 = 0.59 s fill Round gate: d_s = ∛(32 × 80,000 / (π × 40,000)) = ∛20.37 = 2.73 mm (> 2.5 mm wall) Freeze ratio (1.75 / 2.5)² = 0.49 of the wall's freeze time

The Menges equations give a 1.75 × 3.30 mm gate. At a 0.5 s fill, though, the shear rate in that gate is about 19 % over the polycarbonate limit. Either widen the gate to at least 3.92 mm, or slow the fill to about 0.59 s, or both. The round-gate line shows why a tunnel gate is a poor fit for this part: a round gate would need to be at least 2.73 mm across to stay under the limit, larger than the 2.5 mm wall it feeds, so it would leave a big vestige and freeze after the wall. Two smaller gates, each filling half the volume, would be another way out. Press Load the worked example to see the calculator reproduce these numbers.

Gate shear rate versus gate width for the worked example Line chart of apparent shear rate against gate width, for an 80,000 cubic mm per second flow through a 1.75 mm deep gate. Shear rate falls as 1 over W: about 78,400 per second at 2 mm, 52,200 at 3 mm, 39,200 at 4 mm, 26,100 at 6 mm and 19,600 at 8 mm. A dashed line marks the 40,000 per second polycarbonate limit. The Menges width of 3.30 mm sits above the line at 47,500. The line is crossed at 3.92 mm, the shear-safe width. 020,00040,00060,00080,000 gate shear rate (1/s) 2345678 gate width W (mm), depth fixed at 1.75 mm PC limit 40,000 1/s over the limit: risk of splay, burns, degradation Menges W 3.30 mm → 47,498 shear-safe W 3.92 mm
Figure 2. The worked example drawn to scale. For a fixed depth, shear rate falls in proportion to 1/W, so a modest widening fixes a modest overshoot. Making the gate deeper is more powerful (shear falls with 1/h²), but depth is capped by the wall: going deeper than about 0.9 t delays gate freeze until after the part.

Common mistakes

Three gate types compared: edge, overlap and tunnel Three side sections. Left: an edge gate, a thin rectangular channel entering the part edge at the parting line, trimmed after molding. Middle: an overlap gate, where the gate runs onto the face of the part by a length L2 equal to h plus W over 2, which spreads the flow and reduces jetting. Right: a tunnel or submarine gate, a round conical channel that enters the part below the parting line and is sheared off automatically when the part is ejected. Edge gateOverlap gateTunnel / submarine gate simple to cut and adjust vestige on the part edge needs trimming L2 = h + W/2 flow hits the cavity wall first: reduces jetting vestige on the part face part round tip d sheared off at ejection no trimming; d limited by wall and shear runner runner
Figure 3. The calculator covers these three gate types. Edge and overlap gates are rectangular and use the Menges depth and width; the overlap gate adds L2. Tunnel and pin gates are round and are sized here only by the shear limit and the wall they feed. Dashed line = parting line.

When to use this calculator vs other methods

MethodUse it whenLimit
Menges equations plus shear check (this page)Concept design, quoting, reviewing a gate someone has proposed, picking a first-cut steel-safe sizeEmpirical; ignores flow length, gate location, weld lines and non-Newtonian effects
Resin supplier gate guidelinesA specific grade, especially filled, flame-retardant or heat-sensitive gradesUsually given as ranges (for example a fraction of the wall), not a formula with area
Mold-flow simulationThin walls, long flow lengths, multiple gates, cosmetic parts, tight tolerancesNeeds a near-final model and the grade's material data; the result is still checked at the first trial
Trial and open-up at the first sampleAlways, as the final step: gates are cut steel-safe and opened in small stepsEach change is a tool modification, so start close to the right size

Fan gates and film gates, which spread the flow across a wide, flat part, are a variation on the edge gate: their depth at the part follows the same h = n·t rule, but the width is set by the part edge rather than by the area formula. Hot-runner valve gates are sized by the hot-runner maker's nozzle range, so this page is not the right tool for them; their shear check is the same round-gate formula.

Design tips specific to gates

Questions and answers

How do you calculate the gate size for an injection mold?

For a rectangular edge gate, a widely used method from Menges, Michaeli and Mohren sets the gate depth to h = n × t and the gate width to W = n × √A / 30, where t is the wall thickness at the gate in mm, A is the surface area of the cavity in mm² and n is a resin constant from 0.6 to 0.9. Example: polycarbonate (n = 0.7), a 2.5 mm wall and 20,000 mm² of surface give h = 1.75 mm and W = 3.30 mm. Then check that the shear rate in the gate stays below the resin limit at your fill rate.

What is the n factor in the gate size formula?

n is a material constant in the Menges gate equations. The published values are 0.6 for polyethylene and polystyrene, 0.7 for acetal, polycarbonate and polypropylene, 0.8 for cellulose acetate, acrylic and nylon, and 0.9 for PVC. Resins that are more viscous or more shear and heat sensitive get a larger n, which means a deeper, wider gate. Resins not in the original table, such as ABS, need an assumed value; this calculator uses 0.7 for ABS and labels it as an assumption.

Which surface area A goes into the gate width formula?

A is the surface area of the cavity the gate fills, which is the outside surface area of the molded part, in mm². CAD software reports it directly. It is not the projected area used for clamp tonnage. If one part has two gates, give each gate the area it fills. Because W grows with the square root of A, doubling the area widens the gate by only about 41 percent.

How do I know if my gate is too small?

Check the shear rate. For a rectangular gate the apparent shear rate is 6Q / (W·h²), where Q is the volume flow rate through the gate in mm³/s. For a round gate it is 32Q / (π·d³). Compare the result with the maximum shear rate for your resin, for example about 40,000 1/s for polycarbonate and about 100,000 1/s for polypropylene in common simulation databases. Above the limit, the melt can degrade, and you may see splay, burn marks or jetting near the gate.

Why should the gate be thinner than the wall?

The gate must freeze after the part has been packed but before the screw pulls back, so that melt cannot flow back out of the cavity. A gate depth of 0.6 to 0.9 times the wall does that, and it leaves a small vestige that is easy to trim. Conduction cooling time scales with thickness squared, so a gate at 0.7 t freezes in roughly half the time of the wall. A gate much thinner than that freezes too early, which stops packing and leads to sink and voids.

How long should the gate land be?

As short as the tool steel allows, typically about 0.5 to 1.0 mm. Pressure drop through the gate rises in direct proportion to land length, and a long land also freezes sooner. A short land gives a clean break or trim line at the part.

Should the gate be cut to the calculated size straight away?

Many toolmakers cut gates slightly smaller than the calculated size and open them up after the first trial, because removing steel is easy and adding it back is not. That is called keeping the gate steel-safe. The exception is when the shear check shows the calculated gate is already at or over the resin limit: then start at the shear-safe size.

Ask JCH about your gate

Not sure where to gate, or whether an edge or tunnel gate suits your part? Ask our AI assistant. It answers from this website, and our tooling team follows up if you want.

AI assistant. Answers can be wrong; nothing it says is a quote or a promise.

Want a gating plan for your part?

This calculator gives an engineering estimate. Our tooling team reviews your part, resin and appearance needs, and recommends gate type, location and size together with the runner.

Book a 30-min call Send a drawing or sample