Polypropylene, polyethylene, PEEK and PVDF resist the widest range of acids, bases and alcohols. Nylon and acetal handle fuels, oils and many solvents but not acids. PC and ABS are the weak pair against solvents, ketones and chlorinated cleaners. Read every chart rating as an unloaded specimen soaked at room temperature, then test your exact grade.
A chemical resistance chart is a grid: resins across the top, chemicals down the side, and a rating where they cross. The patterns below come from two broad charts that cover most of the resins buyers ask about: the stock-shape maker Ensinger's table, tested at 23 °C, and Thermo Fisher's labware summary built on Nalgene data at 20 °C. Victrex's PEEK guide and Arkema's Kynar PVDF chart fill in what happens with heat and concentration.
Here are the rows behind those statements. Ratings are Ensinger's, for unloaded stock-shape material at 23 °C. Ensinger's own key says each symbol also depends on concentration, time and temperature.
| Family: chemical | PP | PE | POM-C | PA6/66 | PC | PET/PBT* | ABS | PEEK | PVDF |
|---|---|---|---|---|---|---|---|---|---|
| Acid, dilute: hydrochloric 2% | + | + | – | – | + | + | + | + | + |
| Acid, conc.: hydrochloric 36% | + | + | – | – | o | – | + | + | + |
| Acid, conc.: sulfuric 98% | + | o | – | – | – | – | – | – | o |
| Base: sodium hydroxide 5% | + | + | + | + | – | o | n/l | + | o |
| Base, conc.: sodium hydroxide 50% | + | + | + | o | – | – | + | + | o |
| Alcohol: isopropanol | + | + | + | + | – | o | o | + | + |
| Alcohol: ethanol 96% | + | + | + | o | o | + | + | + | + |
| Aliphatic: heptane, hexane | + | – | + | + | + | + | + | + | + |
| Aromatic: toluene | + | o | + | + | – | o | – | + | + |
| Ketone: acetone | + | + | + | + | – | o | – | + | o |
| Ketone: MEK | o | o | o | + | – | o | – | + | o |
| Chlorinated: methylene chloride | – | o | o | o | – | – | – | + | + |
| Chlorinated: trichloroethylene | o | o | – | o | – | – | – | + | + |
| Fuel: diesel oil | o | + | + | + | o | + | + | + | + |
| Oil: silicone oils | + | + | + | + | + | + | + | + | + |
| Water: warm | o | o | o | o | o | – | + | + | + |
Key: + resistant, o conditionally resistant, – not resistant, n/l not listed. *Ensinger reports PET and PBT as one column. PA6 and PA66 are separate columns in the source but carry identical ratings on every row shown. POM-C is acetal copolymer; the homopolymer (POM-H) rates lower in several rows, including a minus for 5% sodium hydroxide where the copolymer has a plus. Ensinger's chart says PE, not HDPE specifically.
If your shortlist is still open, the broader trade-offs are on choosing the right resin and the plastic material selector. For the PC, ABS and PP triangle in particular, see ABS vs polycarbonate vs polypropylene.

No two publishers use the same scale, so the first job is reading that chart's key. The four we opened for this page show the range:
Other charts use four letters or numbers. Whatever the scale, a rating is a summary of one test on one material: a specimen, a chemical at one strength, one temperature, one exposure time and a pass rule chosen by the publisher. It does not tell you about your grade, your color, your part's stress or the cleaner your end users will actually buy. A blank cell means nobody tested that pair; it is not a quiet pass.
Put two charts side by side and some cells contradict each other. These are from the sources cited here:
| Resin | Family | Thermo Fisher, 20 °C | Ensinger, 23 °C | Resin maker |
|---|---|---|---|---|
| PVDF | Chlorinated solvents | N for halogenated hydrocarbons | + for methylene chloride and trichloroethylene | Arkema: Kynar homopolymer to 50 °C in methylene chloride, 140 °C in trichloroethylene |
| Nylon | Alcohols | N for aliphatic alcohols | + isopropanol, o ethanol 96% | Not checked here |
| PC | Alcohols | G for aliphatic alcohols | – isopropanol, o ethanol 96% | Not checked here |
| HDPE / PE | Aliphatic hydrocarbons | G | – heptane and hexane | Not checked here |
| PP | Aromatic hydrocarbons | F | + toluene | Not checked here |
Some of the gap comes from what each publisher measured. A family row on a summary chart covers every member of that family, so a single aggressive solvent can set the letter for all of them, while a single-chemical row speaks only for that chemical. The keys differ too: Thermo Fisher grades by damage over a fixed exposure period on labware resins, Ensinger by its own three-step scale on stock shapes, and the specimens, grades and pass rules are not the same. Neither chart explains individual cells, so don't try to pick the more convenient answer. A disagreement goes on the test list. Where the resin maker publishes its own chart, as Arkema does for PVDF, that is the closest you'll get to data for the actual material, and it's still for their grades, not every PVDF on the market.
A plus at room temperature is not a plus at 80 °C. Ensinger notes that most diffusion processes speed up with temperature, which is why its ratings only hold for the test conditions. Victrex's PEEK chart shows the slope cleanly: methyl ethyl ketone rates A at 23 °C, B at 100 °C and C at 200 °C, and ethylene glycol goes from A at 100 °C to B at 200 °C. Ensinger's water rows show the same thing at a lower level, with six of the nine resins losing at least one step between cold and warm water.
Concentration works the same way. Arkema's Kynar chart drops the homopolymer's maximum use temperature in acetic acid from 110 °C at 10% to 95 °C at 50% and 65 °C at 80%. Sulfuric acid runs from 120 °C up to 60% strength to 50 °C at 94 to 98%. Acetone diluted to 10% in water is listed to 50 °C; at 11 to 25% the limit falls to 25 °C; neat MEK is NR. In Ensinger's table, raising hydrochloric acid from 2% to 36% moves PC from a plus to conditional and PBT from a plus to a minus.
Mixtures are their own problem. Ensinger states that it is generally not possible to reliably predict how a mixture will behave, and gives aqua regia as the extreme case: hydrochloric and nitric acid mixed 3:1, which only PVDF can handle long term, and only at 20 °C, even though many plastics resist each acid alone. Most cleaning products are blends, so a chart row for one ingredient is only a hint.
Grade matters inside a single resin family. Arkema rates its Kynar homopolymer NR in sodium hydroxide up to 10%, while two of its Kynar Flex copolymers are listed to 25 °C and 50 °C in the same solution. Ensinger notes that glass-fiber reinforced grades show slightly lower resistance to strong alkalis than unfilled grades, which is worth remembering before assuming a glass-filled grade inherits the unfilled chart. The acetal pair shows it too: Ensinger gives the copolymer a pH range of 4 to 13 and the homopolymer only 4 to 9. The comparison on nylon vs acetal covers how those two families differ in service.
The diagram plots Ensinger's room-temperature pH limits. PC and ABS are not in that pH table, so they are left off rather than guessed. For PEEK, PPS, PEI and other hot-service resins, the chemistry at temperature is covered in more depth on high-temperature plastics.
None of the charts above builds in a sustained load: Victrex immersed free test bars, and the others state no strained-test condition. ISO 175, the immersion method, says so in its scope: specimens are free from external restraint, and environmental stress cracking is left to the ISO 22088 series. Ensinger adds a specific warning about amorphous resins in chemicals that can cause stress cracks, and Arkema notes that some combinations of chemical and mechanical load crack materials that are otherwise resistant. A molded part with a press-fit pin, a thread-forming screw or a latch that sits deflected is not the specimen in the chart. If any feature carries sustained strain where the chemical lands, read the chart as a first screen only and see environmental stress cracking for how that failure works and how it is tested.
When a part's life depends on the answer, test the exact grade and color you'll mold, with your chemical at its real strength and temperature. Two standards cover unstressed exposure:
The arithmetic is simple. Weigh and measure each specimen before exposure, then again after. Weight change in percent is (mass after − mass before) ÷ mass before × 100. Property retention is the exposed value ÷ the control value × 100, using unexposed bars from the same lot as the control. Neither standard tells you what result counts as a pass for your product, so write the limits into the test plan before the first bar goes in the jar.

Take a hypothetical handheld instrument housing. The cleaning instructions call for 70% isopropyl alcohol wipes and, now and then, a 0.5% hydrogen peroxide disinfectant, both at room temperature. The team is weighing six resins: PC, ABS, PBT, PP, acetal copolymer and nylon 6.
Step 1: screen on the charts. Ensinger lists isopropanol and 0.5% hydrogen peroxide directly; Thermo Fisher adds a family rating for aliphatic alcohols on three of the six. Ensinger's PBT ratings are its combined PET/PBT column.
| Resin | Isopropanol (Ensinger) | Hydrogen peroxide 0.5% (Ensinger) | Alcohols (Thermo Fisher) | Screen result |
|---|---|---|---|---|
| PC | – | + | G | Charts disagree; test only if PC is required |
| ABS | o | + | Not listed | Test |
| PBT | o | + | Not listed | Test |
| PP | + | + | E | Test to confirm |
| Acetal copolymer | + | + | Not listed | Test to confirm |
| Nylon 6 | + | – | N | Drop |
Nylon drops out on the peroxide. PC is held back because one chart fails it in isopropanol, and the cleaner itself is a 70% alcohol and water mixture, which no chart row matches exactly. That leaves four to test.
Step 2: set the pass rule first. This team writes its own limits for the alcohol soak: weight change under 0.5%, at least 90% of the control bars' break load retained, and no visible change in gloss or color. These are the hypothetical team's choices for this product, not values from either standard. Specimens are molded from the exact grades and colors and soaked 168 hours at 23 °C in the actual wipe solution.
Step 3: run the numbers. Illustrative results, not data for any real grade:
The peroxide set runs the same way with its own specimens. Three resins survive the unstressed soak, but this housing has screw bosses and a battery-door latch, so the survivors still need a strained test before anyone approves the cleaning instructions. After that, the pick among PBT, PP and acetal comes down to stiffness, appearance, tolerance and cost, and the cleaner list and resin grade both go on the drawing. If the product is a medical or food-contact item, also read food-safe and medical-grade molding before locking the grade.
It means the material showed some effect under the publisher's test, so it might work and it might not. Thermo Fisher's F, for example, means some effect after 168 hours of constant exposure, which can be cracking, crazing, strength loss or discoloration. Treat any middle rating as a test item, not an approval, and check whether short contact or a lower temperature changes the picture.
In the table above, PVDF has no minus rating and PEEK only one, but neither is universal. Ensinger rates PEEK not resistant to 98% sulfuric acid and 40% hydrofluoric acid, and Arkema lists methyl ethyl ketone as not recommended for its Kynar PVDF. For room-temperature acids and bases, polypropylene earns a plus on most of the same rows.
Treat the blank as unknown, not as safe. Ask the resin supplier whether it has data for that chemical on your grade, look for the closest listed chemical only as a hint, and then test molded specimens in the actual product at its real concentration and temperature. Ensinger notes that mixtures generally can't be predicted from their ingredients, so test the blend itself.
It can. Ensinger notes that glass-fiber reinforced grades show slightly lower resistance to strong alkalis than the same resin unfilled. Fillers, impact modifiers, colorants and flame retardants all change the formulation, so a chart for the unfilled base resin is a starting point. Use the resin maker's data for the filled grade, or test it.
Usually for oils, less so for fuels and solvents. Ensinger rates PP conditional and PE resistant in diesel, PE not resistant in heptane and hexane, and both conditional or worse in methylene chloride and trichloroethylene. Thermo Fisher notes the swelling these solvents cause in PP and HDPE is normally reversible, but a swollen part can still lose fit or stiffness while wet.
Send the part file and the quantity you expect to run, and we'll review it before you commit to tooling. NDA first if you want one.
Send a part for reviewBook a 30-minute call