Rotational Molding Shot Weight Calculator
How much powder for my rotomolded wall thickness? Multiply the mold surface the plastic will line by the nominal wall and by the density of the solid resin: shot weight ≈ A × t × ρ. A 30 in × 49 in closed LLDPE tank with a 3/16 in wall comes to about 38 lb by that rule, taking 0.939 g/cm³ for the resin; the catalog lists that tank at 42 lb, so read the result as a lower bound. For polyethylene, the Association of Rotational Molders says small and medium parts often run 0.125 to 0.250 in (3.2 to 6.4 mm) and warns about walls under roughly 0.075 in (1.9 mm). Enter an area, or the outside dimensions of a box, tank or ball, and the calculator also gives the exact shell weight, the inside capacity and whether the loose powder fits in the mold.
Engineering estimate for planning, not a quote. A × t × ρ assumes the wall is even; the molder's first weighed charges and sectioned parts settle the real number.
How this works
A rotational mold is a hollow metal shell with no core. A weighed charge of resin powder goes in, the mold closes, and it turns on two axes inside an oven. Wherever the metal gets hot enough, powder sticks and builds up, until, as the ARM chapter on wall uniformity describes it, the loose pool is fully depleted and all of it is adhered to the wall. Every gram of the charge ends up in the part, so the arithmetic is a volume balance: the plastic you put in equals the area it spreads over times how thick it lies.
Why proportional is the right model. The ARM design guide's chapter on nominal wall thickness states that wall thickness is altered by changing the shot weight put into the mold and that an increase in shot weight creates a proportional increase in nominal wall thickness. It defines the nominal wall as the average the designer assumes around the part. So A × t × ρ is not a rule of thumb laid on top of the process; it is the process's own bookkeeping, with one simplification: it treats the outer and inner faces of the wall as the same size.
Which area to enter. Use the outer surface of the part, which is the inside surface of the mold. If a panel is molded closed and trimmed out later, its area still takes powder and belongs in A. If a patch of the mold is insulated so nothing builds up there, which LyondellBasell's rotational molding guide gives as a way to form openings, leave that area out. A CAD package gives the surface area directly; for anything close to a box, cylinder or ball, the shape options here are quicker.
Which density to enter. The density that matters is that of the finished, fully fused plastic, the figure a resin datasheet reports. The ARM chapter on wall separation and bridging notes that powder bulk density is likely to be roughly one third of the molded density. Entering a bulk density would make the charge about three times too small. The bulk figure has its own use, in the powder room check below.
Published wall-thickness guidance
We found no standard that fixes the wall of a rotomolded part. What exists is guidance from the trade association, a resin maker and a design magazine, nearly all of it written for polyethylene. The calculator compares your wall with the rows below.
| What is stated | Figure | Source |
|---|---|---|
| Polyethylene nominal walls for small and medium parts | often 0.125 to 0.250 in (3.2 to 6.4 mm), called a good compromise between strength, cycle time, ease of processing and cost | ARM, nominal wall chapter |
| Large parts | made with much greater walls, up to two-plus inches (over 50 mm) | same chapter |
| Thin-wall caution | below approx. 0.075 in (1.9 mm), areas may be inadequate or even zero thickness; specify a minimum wall | same chapter |
| Overall range in one resin maker's guide | 1/32 in to 1 in (0.8 to 25 mm) | LyondellBasell guide |
| Section-to-section variation, not counting corners | about ±20% in normal commercial molding; about ±10% with tighter process optimization, at extra development cost and scrap | ARM, wall uniformity chapter |
| Corners | walls thicken gradually on outside corners and run slightly thinner on sharp inside corners | same chapter |
| Parallel walls (double-wall parts) | 5 × nominal wall apart, outside surface to outside surface, recommended; 3 × molded with only occasional bridging | ARM, wall separation chapter |
| Corner radii | inside at least 1/8 in, outside at least 3/16 in; walls over 3/16 in need an outside radius at least equal to the wall, and the inside radius rises by the same amount | Machine Design, May 2000 |
Two of these disagree at the thin end. LyondellBasell's guide lists 1/32 in as possible, while ARM flags anything under about 0.075 in as a risk of bare spots. The calculator shows both rather than choosing. Between 0.075 in and 0.125 in neither source gives a verdict, so labeling that band "workable with a stated minimum wall" is our reading. For the inside corner radius on walls over 3/16 in, the calculator takes "rises by the same amount" to mean 1/8 in plus the wall's excess over 3/16 in; that arithmetic is also our reading of the article. They also differ on spread: LyondellBasell's guide says wall uniformity can be held within ±10 percent, while ARM expects about ±20% in normal commercial molding and ±10% only with tighter optimization; the calculator reports ARM's two figures.
Resin density presets
Density moves the answer in direct proportion, so a preset is only a starting point. Each one below is a single named rotomolding grade from a datasheet or grade table we retrieved; use your own grade's figure once you have it.
| Preset | Value used | Where it comes from |
|---|---|---|
| LLDPE | 0.939 g/cm³ | SCGC M9001RW datasheet, density by ASTM D 1505; the sheet lists the grade for large tanks and thick-wall parts |
| HDPE | 0.945 g/cm³ | CPChem rotational molding grade table, Marlex HMN TR-945 (the same table lists TR-942 at 0.943) |
| PP copolymer | 0.900 | LyondellBasell Icorene grade range, grade 4014; the table prints densities without a unit, and reading them as g/cm³ is ours |
| Nylon (PA6) | 1.110 g/cm³ | Matrix Polymers Revolve PA RDN datasheet, ISO 1183 on rotomolded specimens; the Icorene table above lists its PA6 grade 7710 at 1.150 |
Polyethylene naming varies by supplier. ARM's materials chapter says rotomolding grades are normally under 0.940 g/cm³ when called LLDPE and over 0.940 when called HDPE, while CPChem files its 0.936 and 0.939 grades under MDPE. The label matters less than the number on the sheet.
Worked example 1: a published 130-gallon tank, checked against its catalog weight
Press Load example: 130-gallon LLDPE tank to reproduce this. A catalog listing for a Tamco 130-gallon vertical tank gives LLDPE, 30 in diameter, a 3/16 in wall and a weight of 42 lb. Its specification table lists the height as 49 in while its title says 47 in; we used 49. The resin grade is not given, so the LLDPE preset of 0.939 is our assumption, and the tank is modeled as a flat-ended cylinder.
Running the two smaller tanks in the same series the same way: the 40-gallon tank (19 in × 41 in, 3/16 in wall, listed at 24 lb) works out to 19.17 lb, and the 75-gallon tank (24 in × 45 in in its table, 3/16 in wall, listed at 35 lb) to 27.34 lb. All three estimates come in below the catalog figures: A × t × ρ by 8.7, 20.1 and 21.9 percent, and the exact-shell figure the calculator headlines by 9.6, 21.3 and 22.9 percent. The listings do not say whether the weight is the bare tank or includes the lid, fitting and packaging, or whether 3/16 in is a nominal or a minimum wall. Our reading is that most of the gap comes from those items and from the domed top and molded features a flat-ended model leaves out; ARM's ±20% spread cannot explain it alone, because that spread runs both ways. So the formula gets the order of magnitude right but ran low on every tank we checked: treat the result as a floor, plan material above it until weighed trial parts exist, and confirm the charge with the molder. The thin-wall tanks also show that the exact-shell correction barely matters at this wall.
Worked example 2: a closed HDPE box
This is an illustrative design, not a published part. The wall sits at the thick end of ARM's common range, the powder takes about a quarter of the cavity, and the exact shell trims a little under 3 percent off the simple estimate.
Worked example 3: a small nylon ball, where the shortcut breaks down
Press Load example: 100 mm nylon ball. A float or ball 100 mm across with a 6 mm PA6 wall (ρ = 1.110 g/cm³):
Two things go wrong at once on a small, thick part. The inner face is much smaller than the outer one, so A × t overstates the plastic by 13 percent. And the loose powder all but fills the mold before any heat goes in, which is the situation ARM warns about: with a cavity this small relative to the charge, it says powder flow may be retarded enough to cause bridging and excessive wall variation. The ball is our illustration, not a published case. The calculator also raises a caution once the powder would take more than half the cavity; that one-half line is our reading, since ARM gives no figure.
After the first parts: adjusting the charge
Because the outside of the part is the only face set by metal, the wall can be changed after the mold exists. ARM's nominal-wall chapter points out that this lets a design be thickened or thinned after in-use testing, and that for many non-structural items a nominal wall is assumed in the design knowing it can move once the mold is available. Two side effects come with a heavier charge, both noted in the same chapter: a larger shot lengthens melting and sintering and may lengthen cooling, and a thicker wall shrinks the internal volume, which can matter for a small tank sold by capacity. The calculator's inside-capacity line shows that second effect for the box, tank and ball shapes.
When you write the drawing, pair the nominal wall with a minimum wall. ARM recommends this as the molder's inspection limit, and with ±20% variation in normal molding, a 6 mm nominal can be expected to read anywhere from about 4.8 to 7.2 mm across wall sections, with corners excluded. Its wall uniformity chapter also explains where the spread comes from: uneven heating is usually the main cause, areas shielded from heat come out thinner, and molders use heat fins, air amplifiers or insulation to steer it.
Common mistakes
- Using the powder's bulk density. It is roughly a third of the molded density, so the charge comes out about three times too light.
- Entering the thinnest acceptable wall as t. The formula wants the average; the minimum belongs on the drawing as a separate limit.
- Leaving out trimmed panels. A section molded closed and cut away later still takes its share of powder.
- Trusting A × t on a small, thick part. Check the exact shell; on the 100 mm ball it is 13 percent lighter.
- Copying polyethylene wall ranges onto other resins. The published ranges are stated for polyethylene, and ARM advises checking whether a specialty material has a maximum recommended wall.
- Forgetting the powder has to fit. On compact parts, compare three times the molded volume with the cavity before the mold is designed.
Where this estimate fits, and what to reach for instead
| Approach | Best for | Limitation |
|---|---|---|
| This calculator | Concept stage: a first charge weight, a sanity check on a supplier's figure, a quick capacity or powder-room check | Even wall assumed; simple shapes only for the exact check |
| CAD mass properties | Real geometry with ribs, kiss-offs and recesses; Machine Design notes solid models give exact part weights and show whether the powder will fit | Needs a shelled model at the right wall |
| Weighed trial charges on the real mold | Final shot weight and wall, measured on sectioned parts | Needs the mold built |
| Part weight from volume | Any part where you already know the plastic volume | Does not derive volume from a wall |
Sources for the method. Proportional shot weight and wall, nominal and minimum wall, the 0.125–0.250 in, 0.075 in and two-plus-inch figures, cycle and capacity effects: ARM Design Guide, Nominal Wall Thickness & Wall Thickness Limits. ±20% and ±10% variation, corner thickening and heating effects: ARM, Wall Thickness Uniformity. Bulk density about one third of molded density, powder room, and 5 × / 3 × wall separation: ARM, Minimum Wall Separation & Bridging Defects. LLDPE and HDPE density naming: ARM, Common Plastic Materials. 1/32 to 1 in range, ±10 percent, insulated openings: LyondellBasell, A guide to rotational molding. Corner radii and CAD weights: Machine Design (2000). Densities: SCGC M9001RW, CPChem Marlex, Icorene grade range, Revolve PA RDN. Tank dimensions and weights: catalog listings for the 40, 75 and 130 gallon Tamco tanks. Unit factors (in, in², ft², lb, gal, lb/in³): NIST SP 811, Appendix B.8. The exact-shell formulas, the powder-fill check and the cube and sphere curves are our own geometry. All of the pages and datasheets listed here were fetched and read on November 20, 2026.
Reviewed by the JCH tooling team · updated November 2026.
Questions and answers
How do I work out how much powder to put in a rotational mold?
Multiply three numbers together: the area of mold surface the plastic will coat, the wall you are designing to, and the solid density of the resin. With square centimeters, centimeters and grams per cubic centimeter the answer comes out in grams. Against the exact geometry of a closed box or tank that product runs a touch heavy, since the inner face of the wall has less area than the outer one; against the listed weights of real tanks it came out light, so use it as a starting figure.
What wall thickness is normal for a rotomolded polyethylene part?
The rotational molders' trade association puts most small and mid-size polyethylene parts at roughly an eighth to a quarter of an inch, about 3 to 6 mm. It cautions against designing much below 0.075 inch, close to 2 mm, where thin spots become likely, and larger parts have been molded far heavier than that usual band.
Will the wall come out the same thickness all over?
No. In ordinary production any stretch of wall away from the corners can land about a fifth above or below the nominal figure, and the outer corners build up while tight inner corners come out thin. Extra process development can narrow that spread to around a tenth, but it costs development time and more rejected parts.
Can the wall be changed after the mold is built?
Yes, and that is one of the process's strengths. Only the outer face touches metal, so adding powder thickens the whole part and removing powder thins it, with no change to the tooling. Trial parts at one charge can be followed by a second batch at another. Expect a heavier charge to need more time in the oven.
Should I use the bulk density of the powder or the density of the molded part?
Use the solid density printed on the resin datasheet. Loose powder packs at only around a third of that, so plugging it in would understate the charge roughly threefold. The loose figure is still worth knowing, because it tells you how much room the charge occupies before it melts.
Can the powder charge be too big to fit in the mold?
It can, on compact parts with heavy walls. Loose powder occupies roughly three times the space of the plastic it becomes, so by our arithmetic a ball or cube whose wall is more than about 6 percent of its diameter or side would need more room than the mold offers. A thinner wall, a larger part or another process are the usual ways out.
Do polypropylene and nylon follow the polyethylene wall rules?
Not automatically. The widely quoted wall bands were written with polyethylene in mind, and the trade association suggests confirming whether a specialty resin carries a maximum recommended wall. Density differs too: the polypropylene and PA6 grades we cite list 0.900 and 1.110, so an identical wall weighs about 4 percent less in that polypropylene and 18 percent more in that nylon than in 0.939 polyethylene.
Ask JCH about your rotomolded part
Got a tank, case or float in mind? Put its size, wall and resin into a question and our AI assistant will reply using what this site has published; if it needs a person, a member of our tooling team can take the conversation over.
Replies are machine-generated and can contain mistakes; treat them as pointers, never as pricing or a commitment.
Planning a tank, case or other hollow part?
Send a sketch or CAD file with the resin and the capacity or load it has to meet. Our tooling team will go through the wall, the charge, the corner radii and the gaps between parallel walls with you, and say plainly whether rotational molding still looks like the right process for your volumes.