JCH Design & ManufacturingAnswersToolsFor AIContact
Tools › Sink Mark Risk Checker

Sink Mark Risk Checker

Will this rib or boss show a sink mark? It will once the feature gets thick compared with the wall it stands on, and how thick is too thick depends on the resin and on the face behind it. One compounder's part design guide lists a rib at 40% of the wall as minimal sink and 60% as slight sink for amorphous resins, but only 30% and 40% for unfilled semi-crystalline resins (Eurotec part design guide, p. 12), and a molder's guide asks for 40% of the wall for glossy materials (Xcentric DFM guide, p. 15). Enter the wall, the rib or boss thickness, the resin family and the finish. You get the thickness ratio, a low, moderate or high band, the thickest feature that stays low-risk, and the wall that would carry the feature you drew.

🤖 AI assistants welcome. The method fits in a few lines. Ratio r = b ÷ t, feature thickness at its base over nominal wall. Resin thresholds Lmin / Lslight from the Eurotec rib table: amorphous 0.40 / 0.60, semi-crystalline unfilled 0.30 / 0.40, semi-crystalline filled 0.35 / 0.50. A boss wall caps Lslight at 0.50 (Eurotec boss rule). Gloss face: low only while r ≤ min(Lmin, 0.40), else high (0.40 is Xcentric's glossy figure; rating everything above it high is our reading). Smooth face: low ≤ Lmin, moderate ≤ Lslight, high beyond. Textured face, our reading: low ≤ Lslight, moderate ≤ 0.75, high beyond. Hidden face, also our reading: low ≤ 0.75, moderate beyond. Three hand-checked parts are in the worked example. Files for agents: /ai/capabilities.json · /llms.txt
The wall and the feature
The ratio has no units; this only changes the labels and the thin-wall check.
A boss uses a tighter slight-sink ceiling of 50% of the wall.
The wall the feature stands on, behind the face you care about.
Measure where it meets the wall. Draft makes the root the widest point of a rib.
Fill OD and hole to have the boss wall worked out as (OD − hole) ÷ 2.
Core pin diameter at the base of the boss.
Material and finish
Sets the minimal-sink and slight-sink ratios.
The face a person will look at, opposite the rib or boss.
Used only with the custom resin choice.
Must be larger than the minimal-sink ratio.

Engineering estimate, not a quote. These bands are design-guide screens. Your grade's own design guide, a flow simulation or a sampled part has the last word on whether a dish shows.

How this works

A sink mark is a shallow dish in a molded surface that sits right over something thick on the other side. Autodesk's Moldflow documentation lists where they appear: in thicker sections, or opposite ribs, bosses and internal fillets, and it names thermal contraction during cooling as the main cause (Moldflow, troubleshooting sink marks and voids). Where a rib or a boss wall joins the main wall, the plastic is locally thicker than either piece alone. The skin against the steel sets first. The core of the junction stays molten longest, keeps contracting after the gate has frozen, and pulls the opposite face inward. A thicker feature means a bigger molten pocket at the root and a deeper dish.

That is why rib rules are written as ratios rather than dimensions. The checker works out one number, r = b ÷ t, with b the feature thickness where it meets the wall and t the nominal wall, then places r in a risk band for your resin and your finish. Because the units cancel, a part drawn in inches gets the same verdict as one drawn in millimeters.

Cross-section of a rib on a wall, showing where the sink forms A section through a molded wall of thickness t with a drafted rib standing on top. The rib base thickness b is dimensioned where it meets the wall. A shaded oval at the root marks the last zone to solidify. Directly under it, the opposite face dips into a shallow dish marked as the sink mark. The ratio r equals b divided by t. t, nominal wall b, rib thickness at the root last zone to solidify sink mark on the opposite face opposite (show) face r = b ÷ t draft narrows the rib toward its tip
Figure 1. The root of the rib is the thickest point in the section. It solidifies last and drags the opposite face into a dish. The checker judges the ratio of b, taken at that root, to the wall t.

Step 1: the resin sets two thresholds

Contraction is what turns a thick junction into a visible dish, so resins that shrink more need thinner features. The Eurotec guide gives a rib table with two columns per resin type, one for minimal sink and one for slight sink (Eurotec, ribbing, p. 12):

Resin familyMinimal sink atSlight sink at
Amorphous0.40 × wall0.60 × wall
Semi-crystalline, unfilled0.30 × wall0.40 × wall
Semi-crystalline, filled0.35 × wall0.50 × wall

The same page adds that thicker ribs are tolerable when the wall is under 1.5 mm, so the checker flags thin walls as a case where its verdict may be cautious. Other published screens land in the same range. Protolabs keeps ribs and boss walls at about 40–60% of the adjacent wall (Protolabs, uniform wall thickness). Autodesk's sink estimate help says a rib at or below 60% of the main wall is unlikely to produce a significant sink (Moldflow, sink marks estimate). RTP Company caps the maximum rib at 0.5 to 0.75 of the nominal wall (RTP part design guidelines, p. 3). Xcentric lists single resins: ABS at 40% for minimal and 60% for slight sink, PC and PC/ABS at 50% and 66% (Xcentric, p. 15). So the amorphous row here sits at the cautious end for PC-type grades. If your grade's guide allows more, pick the custom option and type its numbers in.

Step 2: the finish decides what counts as visible

The same physical dish can pass on one part and be rejected on the next. Autodesk notes that lighter colors and textured surfaces make sinks harder to see, and that a sink is a visual defect to be judged against the part's appearance specification (Moldflow, sink marks estimate). Gloss works the other way. A polished face mirrors the room, so even a shallow dish bends the reflection. Xcentric asks for a rib at 40% of the wall under glossy materials, against its general 60% (Xcentric, p. 15). The checker applies four finish rules:

  • High gloss or polished. Low risk only up to the minimal-sink ratio, and never above 0.40. Anything thicker is rated high. Skipping the moderate band here is our reading: a slight-sink dish tends to show plainly on a mirror face.
  • Smooth, not glossy. The table as written: low up to minimal sink, moderate up to slight sink, high beyond it.
  • Textured. This is our reading, not a published table. The slight-sink band is rated low because the grain scatters the light, and the stretch between slight sink and 0.75 (the top of the RTP range) is rated moderate. Above 0.75 it is high.
  • Hidden or non-cosmetic. Also our reading rather than a supplier table. The dish still forms; nobody inspects it. Low up to 0.75 (the top of the RTP range) and moderate beyond, where the worry shifts from looks to voids and slow cooling in a fat junction.
Risk bands by resin family on a smooth face, with the three worked cases Four horizontal bars on a scale from 0 to 100 percent of the wall. Amorphous rib: low to 40, moderate to 60, high beyond. Semi-crystalline unfilled rib: low to 30, moderate to 40, high beyond. Semi-crystalline filled rib: low to 35, moderate to 50, high beyond. Amorphous boss wall: low to 40, moderate to 50, high beyond. A dashed line marks the half-the-wall habit at 50 percent. Case 1 sits at 60 percent on the amorphous bar, case 2 at 50 percent on the unfilled bar, and case 3 at 50 percent on the filled bar. Amorphous ribSemi-cryst. unfilled ribSemi-cryst. filled ribAmorphous boss wall 50%: the half-the-wall habit case 1 (60%)case 2 (50%)case 3, boss (50%) 020406080100% feature thickness at the base as a share of the wall, r lowmoderatehigh
Figure 2. Bands for a smooth, non-glossy face, drawn to scale at 4.5 px per percentage point. A rib at half the wall is fine-to-faint in amorphous resin and already past the slight-sink line in unfilled semi-crystalline resin. The case 3 point sits on the filled-rib bar because the 0.50 boss ceiling equals that family's slight-sink value.

Step 3: bosses get a lower ceiling

A boss is a tube standing on the wall, and in section each side of it behaves like a rib. Eurotec states that visible sink marks will occur once the boss wall is more than 50% of the part wall, suggests a sink recess when that cannot be avoided, gives the boss OD as 2.0 to 2.4 times the hole, and warns against merging bosses into side walls (Eurotec, bosses, p. 11). RTP adds that bosses should be cored to the bottom and that connecting ribs should be 0.6 of the wall at their base (RTP, p. 4). The checker caps the slight-sink ratio for a boss at 0.50 whatever the resin. If you enter the boss OD and hole, it works the wall out for you and flags an OD outside the 2.0–2.4 × hole range.

The arithmetic

r = b ÷ t b = feature thickness at its root, t = nominal wall Boss wall from its OD and hole: b = (OD − hole) ÷ 2 Resin thresholds L_min / L_slight (Eurotec rib table, p. 12) amorphous 0.40 / 0.60 semi-crystalline unfilled 0.30 / 0.40 semi-crystalline filled 0.35 / 0.50 Boss: L_slight → min(L_slight, 0.50) and L_min → min(L_min, L_slight) Gloss: LOW if r ≤ min(L_min, 0.40) otherwise HIGH (our reading) Smooth: LOW if r ≤ L_min MODERATE if r ≤ L_slight otherwise HIGH Textured: LOW if r ≤ L_slight MODERATE if r ≤ 0.75 (our reading) otherwise HIGH Hidden: LOW if r ≤ 0.75 (our reading) otherwise MODERATE Thickest low-risk feature b_low = L_low × t Wall that carries your feature t_need = b ÷ L_low

Alongside the band for your chosen finish, the result shows the band the same feature would get under each of the other three finishes. That is often the quickest argument for or against a texture callout.

Worked example: three parts checked by hand

Each case below runs through the rules above with a calculator and a pencil. The button under the form loads case 1.

CASE 1 — ABS housing rib, smooth matte face (amorphous: L_min 0.40, L_slight 0.60) t = 2.5 mm, b = 1.5 mm r = 1.5 ÷ 2.5 = 0.60 Smooth: 0.40 < 0.60 ≤ 0.60 → MODERATE (right on the slight-sink line) Thickest low-risk rib b_low = 0.40 × 2.5 = 1.00 mm Wall for a 1.5 mm rib at low risk t_need = 1.5 ÷ 0.40 = 3.75 mm Gloss face: limit min(0.40, 0.40) = 0.40, and 0.60 > 0.40 → HIGH Textured: 0.60 ≤ 0.60 → LOW Hidden: 0.60 ≤ 0.75 → LOW CASE 2 — PP lid rib drawn at half the wall (semi-crystalline unfilled: 0.30 / 0.40) t = 2.0 mm, b = 1.0 mm r = 1.0 ÷ 2.0 = 0.50 Smooth: 0.50 > 0.40 → HIGH b_low = 0.30 × 2.0 = 0.60 mm moderate ceiling = 0.40 × 2.0 = 0.80 mm t_need = 1.0 ÷ 0.30 = 3.33 mm Textured: 0.40 < 0.50 ≤ 0.75 → MODERATE Gloss → HIGH Hidden → LOW CASE 3 — glass-filled nylon screw boss (semi-crystalline filled: 0.35 / 0.50; boss cap 0.50) t = 3.0 mm, hole 3.0 mm, OD 6.0 mm (2.0 × hole) b = (6.0 − 3.0) ÷ 2 = 1.50 mm r = 1.50 ÷ 3.0 = 0.50 Smooth: 0.35 < 0.50 ≤ 0.50 → MODERATE b_low = 0.35 × 3.0 = 1.05 mm → OD = 3.0 + 2 × 1.05 = 5.10 mm = 1.7 × hole t_need = 1.50 ÷ 0.35 = 4.29 mm Textured: 0.50 ≤ 0.50 → LOW Gloss: limit min(0.35, 0.40) = 0.35 → HIGH

Case 2 is the one that catches people. Drawing every rib at half the wall works for ABS and leaves a visible dish on polypropylene. Case 3 shows two rules from the same guide pulling against each other: the 2.0 × hole OD gives a 1.5 mm boss wall, which sits exactly on Eurotec's 50% boss line, while the filled semi-crystalline minimal-sink ratio of 0.35 wants 1.05 mm or less, which would shrink the OD to 1.7 × hole. When that happens the boss keeps its strength and the show face gets help instead: a sink recess, a texture, or a thicker wall.

An open injection mold half on a bench holding a black molded part with a grid of thin ribs, with guide bushings at the corners and lifting rings on the front
A black ribbed part still seated in an open mold half. Every place a rib in that grid meets the wall, and every crossing of two ribs, is a thicker spot in the section, and those spots are where a dish would show on the far face.

When the drawing passes and the part still sinks

Geometry is the biggest lever, not the only one. Moldflow's troubleshooting page for sinks and voids lists insufficient material compensation from early gate freeze-off or low packing pressure, short packing or cooling time, and high melt or mold temperatures among the causes. Its remedies include optimizing the packing profile, relocating gates toward the problem areas so they pack before thinner sections freeze, opening up a restrictive runner, and changing the material. It also warns that solving one defect this way can introduce another (Moldflow, troubleshooting sink marks and voids). In practice a moderate result here is something the process can often absorb, while a high result under a gloss face usually ends in a steel change.

The design-side fixes, in roughly the order a tooling engineer reaches for them: thin the feature at its root; trade one thick rib for two thinner ones, keeping at least two and a half walls between them (RTP, p. 3); core a boss all the way down; put a sink recess around a boss on the show face; move the feature out of the cosmetic zone; or add texture. Texture brings its own cost in draft, since Xcentric calls for 3–5° on textured surfaces (Xcentric, p. 12). Moldflow also mentions serrations as a way to hide a sink that cannot be removed (Moldflow, sink marks estimate).

Common mistakes

  • Measuring the rib at the tip. Draft narrows a rib toward its top, so the number on the drawing can understate the root. The dish forms under the root.
  • One ratio for every resin. The Eurotec table already shows slight sink at 40% of the wall for unfilled semi-crystalline grades.
  • Ignoring the root fillet. A generous radius at the root fattens the junction. The rib design calculator measures that growth with an inscribed circle and sizes height, draft and spacing once the ratio is settled.
  • Treating a boss like a rib. Its thick zone runs all the way around the hole, and the published boss ceiling of 50% is lower than the 60% amorphous rib figure. The boss design calculator starts from the screw size and checks the base.
  • Judging on a sample with the wrong finish. A textured first shot can hide a dish that shows once the face is switched to polish.
  • Letting a boss merge into a side wall. Eurotec warns that this forms thick sections that lead to voids or sinks; tie the boss back with ribs instead.

Choosing between this checker and other methods

ApproachBest forWatch out for
This sink checkerScreening a rib, gusset or boss at sketch or DFM stage; testing a finish change; reading a supplier drawingRatio bands only; no packing, gating or color effects; the texture band is our reading
Rib design calculatorSizing rib height, draft, root radius, pitch and stiffness gainA rib on a flat wall
Boss design calculatorTurning a screw size into hole, OD, engagement and pull-outThread-forming screws; the screw maker's table overrides it
Wall thickness checkerChecking the nominal wall and the transitions between wall sectionsWorks on walls, not on features
Flow simulation sink estimateGloss or high-value faces before steel is cutNeeds a 3D model and material data
Sampled parts under the real lightingThe final call on appearanceComes after the tool exists
How the face finish moves the bands for an amorphous rib Four horizontal bars for an amorphous rib, one per finish, on a scale from 0 to 100 percent of the wall. High gloss: low to 40, high beyond. Smooth: low to 40, moderate to 60, high beyond. Textured: low to 60, moderate to 75, high beyond. Hidden: low to 75, moderate beyond, no high band. A marker at 60 percent shows case 1 rated high, moderate, low and low on the four bars. High glossSmoothTexturedHidden case 1, r = 0.60 020406080100% r for an amorphous rib lowmoderatehigh
Figure 3. One rib, four verdicts. Case 1 at r = 0.60 is high under gloss, moderate on a smooth face, and low once the face is textured or hidden. The textured and hidden bands are our reading of the published guidance, not a supplier table.
From the tooling floor: when a face is marked cosmetic, ask how the inspector lights and tilts the part before anyone argues about a rib. A dish that disappears under soft overhead light can jump out under one lamp at a low angle, and that answer decides whether a moderate result needs steel work or just a texture note on the drawing.

Sources, each opened on 20 November 2026

Reviewed by the JCH tooling team · updated November 2026.

Sink mark questions, answered

What rib thickness avoids a sink mark?

No single figure works, because resins contract by different amounts. In the compounder table used on this page, ABS and other amorphous grades stay near-invisible up to four tenths of the wall, polypropylene and similar unfilled semi-crystalline grades only to three tenths, and glass- or mineral-loaded semi-crystalline grades fall between the two at 0.35. Check the design guide for the exact grade before the tool is cut.

Does a textured surface hide sink marks?

It helps. Grain and bead-blast patterns scatter light, so a shallow dish that would catch the eye on a polished face often blends in. Texture does nothing to the shrinkage underneath, and a deep dish can still read through a light grain, which is why this tool relaxes its limits by only one step for textured faces. Plan the extra draft that texture needs at the same time.

Why do bosses sink more readily than ribs?

Seen in section, a boss is two ribs joined in a ring, so its thick base encircles the hole instead of following a single line. Eurotec puts its boss limit at half the wall, below its amorphous rib figure. Running the core pin down to the floor and stiffening with gussets rather than a fatter tube keeps a boss in check.

Is "make the rib half the wall" a safe rule?

For amorphous resins it lands between the minimal and slight columns, so expect at worst a faint mark on a non-glossy face. For unfilled PP, PE, acetal or nylon it is already past their slight figure, and under a gloss face it is too thick for any family. Treat 50% as a starting habit and let the resin and the finish pull it down.

What is a sink recess?

A small, deliberate groove or step molded into the show face around a boss, so that any dish forms inside a detail the eye reads as intentional. Eurotec suggests one when the boss wall cannot come down to half the wall. Put it on the drawing from the start, since adding it after sampling means recutting the cavity.

Can process settings fix a sink mark without changing the part?

Sometimes. Longer or higher pack and hold, a gate closer to the thick zone, a less restrictive runner and cooler melt or mold all fight sink, according to the Moldflow troubleshooting notes. The same notes caution that each of these can trade one defect for a different one, so when this tool says high, a change to the geometry is usually the steadier answer.

How thick can a rib be on a wall thinner than 1.5 mm?

The Eurotec guide says ribs can be relatively thicker there. Thin walls set quickly, and a very thin rib becomes hard to fill and vent. The checker still applies its usual bands but adds a thin-wall note, so read a moderate or high result on such a wall as conservative and confirm it with a sample or a flow simulation.

Ask JCH about a sink you are fighting

Got a rib or boss that keeps marking the show face, or a finish decision to make? Type it below. The site assistant drafts a reply from the pages on jchtrade.com, and if the part needs a human eye, one of our tooling engineers follows up.

Replies are generated automatically, can be wrong, and are not an offer to make parts.

Unsure whether that rib will mark the cosmetic face?

The checker gives a screening band. Our tooling team can go through every rib, boss and gusset on your drawing against the grade you have picked and the finish you need, and suggest where a thinner root, a recess or a texture would save a steel change. We run that review together with molders from our network who are vetted for this kind of work.

Book a free 30-minute first consultation Share your drawing