Answers › Reading a resin datasheet

How do you read a plastic resin datasheet, and which numbers can you trust?

Reviewed by the JCH tooling team · Updated

Read a resin datasheet as a comparison sheet, not a design sheet. Each value is a typical result from a standard molded bar, tested one way, mostly at 23 °C and over minutes. Trust it to rank grades tested to the same standard. For your part, get curves against temperature and time, check moisture state, and test parts.

Start with one real sheet

The sheet used here is SABIC's typical-values datasheet for CYCOLAC MG47F, a general-purpose molding ABS (revision dated 2022-07-21). It lists most properties twice for the same grade, once to ASTM and once to ISO methods, so wherever the columns disagree you are looking at the test, not the plastic. SABIC's LEXAN 141R polycarbonate sheet and DuPont's Zytel 101L nylon sheet fill in what an ABS sheet can't show.

Read the column heading first. SABIC's says typical property values; UL Prospector copies call the same column nominal value. Neither means minimum. The disclaimer at the foot of the sheet leaves suitability to each customer's own testing, so a figure a drawing depends on has to come from a specification the supplier agrees to.

PropertyASTM column (method, condition)ISO column (method, condition)
Tensile modulus2,270 MPa (D638, 5 mm/min)2,370 MPa (ISO 527, 1 mm/min)
Tensile stress at yield44 MPa (D638 Type I, 5 mm/min)47 MPa (ISO 527, 50 mm/min)
Tensile strain at yield / at break2% / 24%2.6% / 25%
Flexural modulus2,300 MPa (D790, 50 mm span)2,200 MPa (ISO 178, 2 mm/min)
Notched Izod, 23 °C320 J/m (D256)22 kJ/m² (ISO 180/1A, 80 × 10 × 4 mm bar)
Notched Izod, −30 °Cnot listed8 kJ/m²
Notched Charpy, 23 / −30 °Cnot listed26 / 9 kJ/m² (ISO 179/1eA)
Heat deflection, 1.8 MPa80 °C (D648, 1.82 MPa, 3.2 mm, unannealed)81 °C (ISO 75/Af, flatwise)
Heat deflection, 0.45 MPa94 °Cnot listed
Melt flow5.6 g/10 min (D1238, 230 °C, 3.8 kg)18 g/10 min (ISO 1133, 220 °C, 10 kg)

Read across each row. One resin, one supplier, yet flexural modulus is 2,300 or 2,200 MPa, impact 320 J/m or 22 kJ/m², melt flow 5.6 or 18. None is a typo. Bar shape, speed, span, load and temperature differ, which is the first rule: a number without its method and condition can't be compared with anything.

Test lab with white cabinets and dark benchtops along both walls, small bench test instruments on the left counter and a white cabinet-style test machine at the back of the room
A product test lab with bench instruments and an environmental chamber. Datasheet numbers come from standard bars in the resin maker's materials lab; testing finished parts, as a lab like this does, is a separate job.

Tensile: modulus, yield and break (ISO 527, ASTM D638)

A dog-bone bar is pulled apart. ISO 527 uses the multipurpose bar, 170 mm long and 4 mm thick; the preferred ASTM D638 bar, Type I, is 165 mm long and 3.2 mm thick. ISO measures modulus at 1 mm/min from the straight first stretch of the curve, between 0.05% and 0.25% strain, then speeds up; MG47F's ISO yield and break values are at 50 mm/min, its ASTM ones at 5 mm/min. Plastics respond to strain rate, and ZwickRoell, which builds the machines, says D638 results should not be compared directly with ISO 527 results.

Three numbers come off the curve. Modulus is stiffness at the very start. Yield is the peak where a ductile resin like ABS starts to neck and stops taking more load; past it a part stays bent, so yield is the practical limit. Break is where the bar finally parts. The diagram plots MG47F's ISO values.

ISO 527 tensile curve for CYCOLAC MG47F ABS. Left: the whole test, rising steeply to yield at 47 MPa and 2.6% strain, then necking and breaking at 35 MPa and 25% strain. Right: the first 3% enlarged, showing the 2,370 MPa modulus line measured between 0.05% and 0.25% strain, the real curve bending away from it, and a 1,808 MPa secant line from the origin to the yield point. Tensile test, ISO 527: CYCOLAC MG47F ABS at 23 °C Curve shape is a sketch; the marked values are the datasheet's. 0 20 40 60 Stress, MPa 0 5 10 15 20 25 Strain, % Yield: 47 MPa at 2.6% part stays bent past here Break: 35 MPa at 25% neck draws out First 3% of strain, enlarged 0 1% 2% 3% modulus 2,370 MPa (slope at 0.05–0.25%) secant to yield 47 / 0.026 = 1,808 MPa The modulus is the slope of the first quarter-percent. By yield the curve has bent over, so near yield a part is about a quarter softer than the headline number.

The enlarged panel shows what most readers miss: the curve bends over long before yield. Divide yield stress by yield strain and you get a secant modulus of 47 / 0.026 = 1,808 MPa, about 24% below the 2,370 MPa printed on the sheet. A snap arm or press fit that works at 2% strain lives on that softer stretch of the curve, so for those parts ask for the stress-strain curve itself, not just the modulus. The snap-fit design page walks through the strain check that goes with it.

Flexural modulus (ISO 178, ASTM D790)

For flexure, a bar rests on two supports and a nose pushes down in the middle. ISO 178 uses an 80 × 10 × 4 mm bar on a 64 mm span. D790's standard molded bar is 127 × 12.7 × 3.2 mm with a span 16 times the thickness, about 51 mm, and the test stops at 5% strain if the bar hasn't broken. ZwickRoell lists the differences as application range, specimen geometry, speed and modulus evaluation, and concludes the results land in the same range without being directly comparable. MG47F shows exactly that: 2,300 MPa by D790 and 2,200 by ISO 178, a 4.5% gap that is pure method.

Most part loads are bending loads, so this is the modulus to use for walls and beams. For an unfilled resin it sits near the tensile value (2,200 against 2,370 MPa here). Bending strains the outer skin hardest, and UL Prospector's guide notes that a molded skin differs from the core, one reason the two results differ. Both were measured along a small bar filled from one end, not across a wide wall.

Impact: Izod and Charpy (ISO 180, ISO 179, ASTM D256)

A pendulum swings through a notched bar and the energy it loses is the result. The unit tells you which family you have. ASTM D256 Izod divides the energy by the bar's thickness and reports J/m or ft·lb/in; its bar is 63.5 mm long and 12.5 mm high with a 45° notch of 0.25 mm radius. ISO 180 Izod and ISO 179 Charpy divide by the cross-section and report kJ/m². Izod grips one end of the bar; Charpy rests it on two supports and strikes the middle. The code 179/1eA on the MG47F sheet decodes as a type 1 bar (80 × 10 × 4 mm) struck edgewise with a notch, which the sheet describes as a V-notch on a 62 mm span.

There is no fixed factor between J/m and kJ/m². Divide the ASTM value by the ISO value on two SABIC sheets and the ratio wanders: MG47F gives 320 / 22 = 14.5, while LEXAN polycarbonate gives 800 J/m (LEXAN 141, ASTM sheet) over 70 kJ/m² (LEXAN 141R, ISO sheet) = 11.4. Don't convert; ask for the value to the method your specification names.

Two more limits. The notch is a standard sharp flaw, so the number ranks notch sensitivity; your part's real corners decide how much toughness you get. And 23 °C is one temperature. MG47F's ISO Izod falls from 22 to 8 kJ/m² at −30 °C, a 64% drop; LEXAN 141R falls from 70 to 12, an 83% drop, though still above the ABS. For parts dropped in the cold, read the cold column, or ask for one.

Heat deflection temperature (ISO 75, ASTM D648)

HDT is the temperature at which a loaded bar, heated at about 120 °C per hour, bends a set amount. ISO 75 Method A stresses the bar to 1.80 MPa and Method B to 0.45 MPa (Method C, at 8.00 MPa, is seldom quoted); ASTM D648 uses 1.82 or 0.455 MPa. ZwickRoell gives the end point as 0.25 mm of deflection for ASTM and 0.20% flexural strain for ISO; ISO turns that strain into a deflection set by bar height and span, about 0.34 mm for the flatwise 80 × 10 × 4 mm bar on 64 mm. The load matters most. MG47F reads 94 °C at 0.455 MPa and 80 °C at 1.82 MPa, so an HDT quoted without its load is half a number.

Setup matters even inside ISO. The 2017 LEXAN 141R sheet tests edgewise on a 120 × 10 × 4 mm bar over 100 mm and reports 125 °C at 1.8 MPa; SABIC's ASTM sheet for the sister grade LEXAN 141 (6.4 mm bar, unannealed) reports 132 °C. MG47F's ISO value is flatwise on the 80 × 10 × 4 mm bar over 64 mm. Compare HDTs only when load, orientation, thickness and annealing match.

HDT is not a service temperature. ZwickRoell calls it a purely comparative value that says nothing about an end product's maximum operating temperature. For long-term heat, the relative temperature index (RTI, UL 746B) is closer to the question: UL ages specimens in hot-air ovens until a property falls to half its original value, then extrapolates a temperature index. MG47F lists RTIs of 80 °C; LEXAN 141R lists 125 to 130 °C. The HDT lookup tool gives representative values for common resins at both loads.

A clear molded part being lifted off the polished core of an open injection mold, with a hand at the right edge
A clear part coming off the core. The photo can't show which resin it is. For clear grades the datasheet adds optical values such as light transmission and haze, each measured at a stated plaque thickness, so a thicker or textured wall needs its own check.

Melt flow rate (ISO 1133, ASTM D1238)

Melt flow rate, MFR (the shop still says MFI), is the mass of melt pushed through a small die in 10 minutes at a set temperature and weight. The conditions are part of the number. MG47F gives 5.6 g/10 min at 230 °C and 3.8 kg to D1238 and 18 g/10 min at 220 °C and 10 kg to ISO 1133. Polycarbonate is tested at 300 °C and 1.2 kg, so LEXAN 141's 11 g/10 min and the ABS's 18 don't say which fills a thin wall better.

The standards admit the limits. ISO 1133-1 notes the test runs at shear rates far below molding, so results may not reflect processing, and calls it chiefly a quality-control method. ASTM D1238 says flow rate is not a fundamental polymer property. Use MFR to compare grades of one family at one condition and to watch lot-to-lot drift. For fill questions, ask for the viscosity-versus-shear-rate curve, which the LEXAN 141 and MG47 ASTM sheets list as multipoint data. Watch the unit too: LEXAN 141R gives a volume rate (MVR, 12 cm³/10 min at 300 °C and 1.2 kg), and converting it to MFR needs the melt density.

Mold shrinkage (ISO 294-4)

ISO 294-4 measures shrinkage on molded test specimens in two directions, parallel and normal to melt flow, and separates molding shrinkage from post-molding shrinkage; its molding figure excludes the effect of humidity uptake. Check the method column before trusting a shrink value. Zytel 101L gives 1.4% along flow and 1.4% across by ISO 294-4. MG47F gives 0.5 to 0.8% along flow on a 3.2 mm bar by “SABIC method”, and LEXAN 141R gives 0.5 to 0.7% on a tensile bar, also by the supplier's own method. A tensile-bar range tells the toolmaker where to start, not what to cut. The mold shrinkage page covers how wall thickness, packing and flow direction move the real figure.

The UL 94 line

A flame class on a datasheet always comes with a thickness. MG47F is HB at 1.5 mm. LEXAN 141R is HB at 0.7 mm and at 3 mm, and the sheet itself points to SABIC's 200 series when a V-2 rating is needed. UL's test page notes that the HB result takes specimen thickness into account. Treat the line as a pointer; the record that counts is the UL Yellow Card, listed in UL's Product iQ database, checked for the exact grade and your thinnest wall. The UL 94 page explains what each class means.

What the sheet leaves out

Most of what decides whether a molded part survives is not on the one-page summary. Four gaps matter most.

Comparable curves are what the CAMPUS database was built for: single-point values to ISO 10350 and multipoint data, such as stress-strain curves, to ISO 11403, on standard specimens. When two candidate grades both have CAMPUS-style data, compare those; otherwise compare like with like, or mold parts and test.

Worked example: one bracket, five readings

Take a hypothetical cantilever tab, 30 mm long, 12 mm wide and 2.5 mm thick, fixed at its root, with 10 N hanging on the tip. Small-deflection beam theory gives the tip deflection as δ = F·L³ / (3·E·I), with I = b·h³ / 12.

Resin and value usedE, MPaTip deflectionRoot strain (24 MPa / E)
CYCOLAC MG47F ABS, ISO 178 flexural modulus2,2002.62 mm1.09%
LEXAN 141R PC, ISO 178 flexural modulus2,3002.50 mm1.04%
Zytel 101L PA66, dry-as-molded, ISO 1782,8002.06 mm0.86%
Zytel 101L PA66, conditioned, ISO 1781,2004.80 mm2.00%
Zytel 101L PA66, conditioned, 1,000 h creep modulus8207.02 mm2.93%

Three things fall out. First, swapping ABS for polycarbonate buys almost no stiffness: 4% less deflection. What PC buys is margin. Its ISO yield strain is 6% against 2.6% for the ABS, so the tab runs at about 17% of yield strain in PC (1.04 / 6) and 42% in ABS (1.09 / 2.6). Second, the nylon's dry and conditioned readings differ by a factor of 2.3; size from the state the part lives in. Third, creep bites under a steady load: the conditioned nylon tab drifts to about 7 mm over 1,000 h, roughly 2.7 times the short-term ABS figure. (Using a tensile creep modulus in a bending formula is an approximation; ask for flexural creep data near a limit.)

Geometry beats resin. Thicken the ABS tab from 2.5 to 3.0 mm and I rises to 27 mm⁴, so deflection drops to 270,000 / (3 × 2,200 × 27) = 1.52 mm and root stress to 1,800 / 108 = 16.7 MPa. Deflection follows the cube of thickness, (2.5 / 3.0)³ = 0.579, a 42% cut. Half a millimeter of wall did about ten times what the resin change did, though a thicker wall raises its own sink and cooling questions. All of this is at 23 °C; in a warm enclosure, rerun it with the modulus from the supplier's temperature curve. The snap-fit calculator runs the same beam check for latch arms, the plastic material selector shortlists families before you open sheets, and ABS vs polycarbonate vs polypropylene compares the everyday three.

Which numbers to trust, and for what

Questions to ask the resin supplier

  1. Is this sheet ISO or ASTM, and can I have the other set for the same grade?
  2. Which properties appear on each lot certificate, and to what limits?
  3. For moisture-sensitive grades: which values are dry-as-molded, which conditioned, and at what humidity?
  4. Can I have stress-strain and modulus-versus-temperature curves covering my service temperature?
  5. Do you have creep data at my stress and temperature, and fatigue data?
  6. For HDT: which load, which bar orientation, annealed or not?
  7. Which UL Yellow Card covers this exact grade, at what minimum thickness?
  8. Is the shrink value ISO 294-4 or your own method, and on what thickness?
  9. Do these values hold for the colored version we will buy?
  10. What drying conditions do you specify? (MG47F: 80 to 95 °C for 2 to 4 h, 0.1% maximum moisture.)

Common questions

Is MFI the same as MFR on a datasheet?

In practice, yes. Melt flow index (MFI) is the shop name for what ISO 1133 and ASTM D1238 call melt mass-flow rate (MFR), in g/10 min. MVR is the volume version, in cm³/10 min. None of them means anything without its temperature and load, such as 230 °C and 3.8 kg for ABS or 300 °C and 1.2 kg for polycarbonate.

Can I convert notched Izod in J/m to kJ/m²?

Not reliably. ASTM D256 divides the break energy by bar thickness, while ISO 180 divides by cross-section, on a different bar. On two SABIC sheets the ratio between the two is 14.5 for an ABS and about 11.4 for a polycarbonate, so any single factor will mislead you. Ask the supplier for the value measured to the method your specification names.

Why do tensile and flexural modulus differ for the same grade?

They come from different tests: a bar pulled evenly versus a bar bent over a span, with different specimens, speeds and strain ranges. Bending loads the molded skin hardest. For unfilled resins the two are close; CYCOLAC MG47F reads 2,370 MPa tensile and 2,200 MPa flexural on its ISO column. Use the one that matches how your part is loaded.

Does a higher HDT mean my part can run hotter?

Only as a ranking. HDT is a short test on a bar loaded to 1.8 or 0.45 MPa, and the test-machine maker ZwickRoell says it gives no information about the maximum operating temperature of an end product. For long-term heat, look at the relative temperature index (RTI) and ask for modulus-versus-temperature and creep data at your temperature.

Are datasheet values minimums I can put on a drawing?

No. SABIC labels its values typical and UL Prospector copies call them nominal. For a property the design depends on, call out the grade by name, agree with the supplier which properties are reported on each lot certificate and to what limits, and test molded parts for anything the certificate does not cover.

Sources

Send the part file and the quantity you expect to run, and we'll review it before you commit to tooling. NDA first if you want one.

Send a part for reviewBook a 30-minute call