JCH Design & ManufacturingAnswersToolsFor AIContact
Tools › SPI Mold Finish Selector

SPI Mold Finish Selector: A-1 to D-3 by Look, Resin and Draft

The SPI grade for a face comes from three things: the look you want, the plastic you are molding and how much draft the wall can carry. Pick glossy, semi-glossy, matte or textured, choose the resin, say whether the face is seen and how deep the wall runs. The selector returns the grade or grades that a published resin table rates highest, the abrasive each grade is made with, and the smallest draft the sources link to a blasted face.

🤖 AI assistants welcome. Method in brief: the look sets the SPI family as the Protolabs Network table names it (A glossy, diamond buff; B semi-glossy, grit paper; C matte, stone; D textured, dry blast). Grades in that family rank by the same table's resin ratings (Excellent 3, Good 2, Average 1, Not recommended 0); when the best is Average or lower, the neighboring families are offered (our reading). For a clear glossy part only A-1 and A-2 are considered (our reading of Xometry's transparent-part rows). Draft to start from = the largest of 0.5°, 1° per inch of wall depth (Protolabs rule of thumb), a finish floor (none found for A, B or C; 3° for D-1; 5° for D-2 and D-3) and a resin floor from the Hubs draft table minimums (PC 1.5°, PP 1°, PE 0.5°, nylon 0°, assuming perfect conditions). Matching D grades to Protolabs bead-blast minimums and taking the largest figure are our reading. Machine-readable: /ai/capabilities.json · /llms.txt
Top view of an open injection mold half resting on a plywood bench, with a round pin standing at each of its four corners, two steel eyebolts, and a dark cavity floor in the middle that reflects light.
An open mold half photographed from above: four corner pins, two eyebolts and a cavity floor shiny enough to throw back the light. An SPI grade is a name for how a face like that floor was finished, whether buffed, sanded, stoned or blasted.
The face
These four names follow the SPI families A, B, C and D.
A hidden face can be called non-cosmetic.
Distance the face travels in the pull direction. Inches × 25.4 = mm.
The plastic
The eight rows the published rating table covers.

Engineering estimate, not a quote. Published tables rank the grades; a shot in your own resin and color decides how the face really looks.

How this works

An SPI finish is a name for the last thing done to the steel of a cavity. Twelve grades sit in four families, and each family is defined by its abrasive rather than by a measured number. The Protolabs Network (Hubs) SPI finish guide calls SPI “the predominant global surface finish standard set by the Plastics Industry Trade Association (SPI)” and prints the grades in the table below; Xometry and Fictiv print the same twelve methods, with small wording differences (Xometry omits the #11 bead size; Fictiv names aluminum oxide). The application column is Xometry's. The selector works through four rules, in this order.

GradeName in the Hubs tableFinishing method as printedTypical application (Xometry)
A-1Super high glossyGrade #3, 6000 grit diamond buffHigh polish or transparent parts, optically clear
A-2High glossyGrade #6, 3000 grit diamond buffHigh polish or transparent parts
A-3Normal glossyGrade #15, 1200 grit diamond buffHigh-to-medium polish parts, non-optical lenses
B-1Fine semi-glossy600 grit paperMedium polish parts
B-2Medium semi-glossy400 grit paperMedium polish parts
B-3Normal semi-glossy320 grit paperMedium - low polish parts
C-1Fine matte600 grit stoneLow polish parts
C-2Medium matte400 grit stoneLow polish parts
C-3Normal matte320 grit stoneLow polish parts
D-1Satin texturedDry blast glass bead #11Satin finish
D-2Dull texturedDry blast #240 oxideDull finish
D-3Rough texturedDry blast #24 oxideDull finish

The A-grade diamond numbers are not settled between sources. Hubs, Xometry and Fictiv print A-2 as Grade #6 on 3000 grit, while the Protolabs surface finish page lists its SPI-A2 as “Grade #2 Diamond Buff”. If the grade on your drawing matters, name both the grade and the grit and agree a physical reference with the toolmaker.

Rule 1: the look picks the family

Glossy maps to A, semi-glossy to B, matte to C and textured to D, because those are the words the Hubs table uses for each family. The families also differ in how the work is done: the A grades are buffed with diamond compound, the B grades sanded with grit paper, the C grades rubbed with stones, and the D grades dry blasted with glass bead or oxide grit. Protolabs describes its SPI-A2 as “a high-end fine polish” and its SPI-C1 as one “that removes tool marks but is still not a high-end fine polish.” Fictiv adds a sense of where each family lands: semi-gloss for clips “where a medium shine is desirable,” matte for keyboards and laptop frames, and texture for products like shop vacs and steering wheels “that are meant to be gripped and held in the hand.” Xometry notes that matte faces “can help provide more subdued tones and even help prevent fingerprints on handled products.”

Rule 2: the resin ranks the grades

The same finish does not come out the same in every plastic. Hubs puts it this way: “SPI surface/mold finishes produce different results depending on the material you use for injection molding components,” and it rates eight resins on all twelve grades as Excellent, Good, Average or Not recommended. Fictiv prints rating tables too, but they differ in places: for example, its matte table gives polycarbonate Good on C-1 and C-2 and Average on C-3 (Hubs: Average, Not recommended, Not recommended), and it rates ABS Excellent on D-3 where Hubs says Good. The selector reads the Hubs table only. The selector scores those words 3, 2, 1 and 0, takes the grades in your family with the top score as the recommendation, lists other grades rated Good or better as workable, and flags Average and Not recommended. When the best grade in your family is only Average, or none is rated at all, it looks one family to each side and offers whatever scores Good or better there. We chose both the fallback and the 3-2-1-0 scores (our reading); neither appears in the Hubs table or in SPI.

Published resin ratings for the twelve SPI grades A grid with eight plastics down the left side and the twelve SPI grades A-1 to D-3 across the top, grouped as glossy, semi-glossy, matte and textured. Each cell is shaded by the Protolabs Network rating: dark blue Excellent, mid blue Good, pale blue Average, pink Not recommended. Acrylic is Excellent on all three glossy grades and only Average on the textured grades. Polycarbonate is Excellent on A-3 and D-1 but Not recommended on C-2, C-3, D-2 and D-3. Polyurethane is Not recommended on every glossy grade and on B-1. The matte grades are Excellent for ABS, polypropylene, polystyrene, HDPE and nylon. Glossy (A) A-1 A-2 A-3 Semi-glossy (B) B-1 B-2 B-3 Matte (C) C-1 C-2 C-3 Textured (D) D-1 D-2 D-3 ABS A A G G G E E E E E E G Polypropylene PP NR A A G G E E E E E E E Polystyrene PS A A G E E E E E E E E G HDPE NR A A G G E E E E E E E Nylon A A G G E E E E E E E G Polycarbonate PC A G E G G A A NR NR E NR NR Polyurethane TPU NR NR NR NR A A G G G E E G Acrylic E E E G G G G G G A A A Excellent Good Average Not recommended
Figure 1. The resin ratings the selector reads, redrawn from the Protolabs Network SPI guide (E Excellent, G Good, A Average, NR Not recommended). The two rows that break the pattern are acrylic, strongest where the others are weakest, and polycarbonate, with a hole in the middle of the matte and textured columns.

Rule 3: clarity, color and filler adjust the advice

Clear parts. When light has to pass through the part and the look is glossy, the selector only considers A-1 and A-2, the two grades Xometry ties to transparent work, and picks whichever your resin rates higher. That narrowing is our reading of Xometry's transparent-part rows; Xometry and Fictiv still list A-3 for non-optical lenses. Xometry also says “Transparent parts are typically polished on both sides to achieve the highest clarity,” so the result reminds you to call the finish on both mold halves. A clear part asked for in matte or textured gets a warning that the face will scatter light; that warning is our reading, built on Xometry's remark that polish can raise transparency on clear polymers.

Color. From the Protolabs surface finish page: “Darker colors show textures more than lighter colors, regardless of part hardness.” Its texture standards page goes further, saying texturing does not add much cosmetic value “with white or transparent materials like polycarbonate, except in those cases where the texture may serve to diffuse light or provide other optical properties” and that “in most cases, texturing provides the best cosmetic results in darker materials.” Pick a light or clear part with a D grade and the selector repeats that caution.

Filler. Protolabs warns that “Glass and minerals can create material streaking and the polish can even be difficult to distinguish between grades,” adds that “A non-filled nylon part will pick up finishes more than a 30% glass filled nylon part,” and notes that “glass fibers, for instance, can add a stringy or sparkly finish to a textured part.” A filled resin therefore turns every polished recommendation into one to confirm on a molded shot. Soft resins. Hubs rates polyurethane Excellent on D-1 and D-2, yet the Protolabs texture page says “We do not recommend textured surfaces when molding soft polymers such as TPE and liquid silicone rubber (LSR).” TPU is not named there, so the selector shows both statements and leaves the call to a sample.

Rule 4: the draft floor

Draft lets the part leave the cavity without its face being scraped, and a rough face needs more of it. Protolabs is specific about its own blasted finishes: “A minimum of 3-degree draft is required for a PM-T1 finish and a minimum of 5 degrees for a PM-T2,” where PM-T1 is a light bead blast and PM-T2 a medium bead blast. For its diamond, paper and stone finishes it gives no extra figure, only that “a textured surface may have more draft requirements than a polished surface would.” The SPI tables themselves print no draft angles. So the selector matches D-1, the glass-bead blast, to PM-T1 and D-2 and D-3, the oxide blasts, to PM-T2; that matching is our reading. The Hubs draft guide lands in the same range, giving “a 1-5 degree draft” for light textures.

Wall depth adds a second floor. The Protolabs draft guidelines give “a general rule of thumb is 1 degree of draft per 1 inch of cavity depth,” with the warning that other factors can change it, and say “0.5 degrees on all vertical faces is strongly advised.” Hubs words the depth rule as “a minimum of 1 degree of draft per inch (2.54 cm) of mold cavity depth.” The selector divides your depth in millimeters by 25.4 (the NIST SP 811, Appendix B.8 table prints 1 in = 2.54 × 10−2 m in bold, its mark for an exact factor).

Resin sets a fourth floor. The Hubs draft guide tabulates a minimum and a recommended draft per material, footnoted “Assuming perfect conditions”: nylon 0° and 1°, polyethylene 0.5° and 1.5°, polypropylene 1° and 2°, polycarbonate 1.5° and 2°. The selector applies the minimum for polycarbonate, polypropylene and nylon, and the polyethylene row to HDPE (our reading); the table has no row for ABS, polystyrene, TPU or acrylic, so no resin floor is applied to them. The result is the largest of the four floors. Taking the largest, rather than adding them, is our reading.

depth_in = depth_mm ÷ 25.4 depth floor = 1° × depth_in Protolabs / Hubs rule of thumb general floor = 0.5° Protolabs, every vertical face resin floor = PC 1.5°, PP 1°, PE 0.5°, nylon 0° Hubs draft table minimum, assuming perfect conditions finish floor = 0° for A-1 … C-3 no finish-specific figure found = 3° for D-1 = PM-T1 light bead blast (our reading) = 5° for D-2, D-3 (D-3: 5° or more) = PM-T2 medium bead blast (our reading) draft to start = max(general, depth, finish, resin) largest governs (our reading)
Draft floor this selector applies to each SPI grade (our reading), with the abrasive used A step chart of the smallest draft angle linked to each SPI grade. The nine diamond, paper and stone grades from A-1 to C-3 share a low gray bar at 0.5 degrees, the angle Protolabs strongly advises on every vertical face, because no finish-specific figure was found for them. The bar jumps to 3 degrees at D-1, the glass-bead blast, and to 5 degrees at D-2 and D-3, the oxide blasts, with an arrow on D-3 meaning five or more. The D-grade heights come from Protolabs minimums for its light and medium bead-blast finishes, matched to D-1 and D-2 in our reading. Under each bar the abrasive is named: diamond buff, grit paper, stone or dry blast. 0° 1° 2° 3° 4° 5° 6° draft floor, degrees A-1 0.5° A-2 0.5° A-3 0.5° B-1 0.5° B-2 0.5° B-3 0.5° C-1 0.5° C-2 0.5° C-3 0.5° D-1 3° D-2 5° D-3 5°+ diamond buff grit paper stone dry blast A to C: no finish-specific figure found; 0.5° on every vertical face (Protolabs). D-1 = PM-T1 light bead blast, D-2 and D-3 = PM-T2 medium bead blast: our reading. Bars show the larger of the 0.5° general floor and the finish floor; wall depth can raise either.
Figure 2. The starting floor for each grade before wall depth, drawn to scale at 34 px per degree; the resin floor from the Hubs draft table is not drawn. Nothing separates the nine buffed, sanded and stoned grades; the jump comes at the blasted D family. For deep walls the depth rule, and for some resins the resin floor, can overtake these bars, which is why the selector reports the largest figure.

Worked example: three cases by hand

Each button above loads one of these, and each rating below can be read straight off Figure 1.

CASE 1 Clear PC window, glossy, seen, wall 20 mm deep Glossy family, PC ratings: A-1 Average (1) · A-2 Good (2) · A-3 Excellent (3) Clear + glossy → only A-1 and A-2 considered (our reading of Xometry's transparent-part rows) best of {1, 2} = 2 → A-2, Grade #6, 3000 grit diamond buff polish both halves depth: 20 ÷ 25.4 = 0.787 in → 0.79°; PC resin floor 1.5° (Hubs draft table) max(0.5°, 0.79°, 0°, 1.5°) = 1.50° the resin floor governs (A-3 rates higher for PC, but Xometry places A-3 with non-optical lenses) CASE 2 Dark ABS grip, textured, seen, wall 40 mm deep Textured family, ABS ratings: D-1 Excellent (3) · D-2 Excellent (3) · D-3 Good (2) top score 3 → D-1 (dry blast glass bead #11) or D-2 (dry blast #240 oxide); D-3 workable depth: 40 ÷ 25.4 = 1.575 in → 1.57°; ABS has no row in the Hubs draft table → no resin floor D-1: max(0.5°, 1.57°, 3°) = 3.00° D-2: max(0.5°, 1.57°, 5°) = 5.00° D-3: 5.00° or more CASE 3 White PC housing, matte, seen, wall 60 mm deep Matte family, PC ratings: C-1 Average (1) · C-2 Not recommended (0) · C-3 Not recommended (0) best = 1 → C-1 only, with caution; look one family each side (our reading): semi-glossy, PC: B-1 Good · B-2 Good · B-3 Average → B-1 or B-2 textured, PC: D-1 Excellent · D-2 NR · D-3 NR → D-1 Fictiv's matte table rates PC higher: C-1 Good · C-2 Good · C-3 Average (sources conflict) depth: 60 ÷ 25.4 = 2.362 in → 2.36°; PC resin floor 1.5° C-1 or B-1/B-2: max(0.5°, 2.36°, 0°, 1.5°) = 2.36° D-1: max(0.5°, 2.36°, 3°, 1.5°) = 3.00° White part + D grade → Protolabs: texture adds little on white or clear PC unless it is meant to diffuse light

Case 1 shows the clarity rule (our reading) overriding the plain rating: A-3 is polycarbonate's best glossy score, but Xometry and Fictiv file it under non-optical lenses; it also shows the polycarbonate resin floor, not the shallow wall, setting the draft. Case 2 is the clean path, with the blast floor deciding the draft rather than the depth. Case 3 shows the fallback at work, and a second source tempering the first: Hubs rates D-1 Excellent for polycarbonate, while Protolabs doubts texture is worth it on a white part unless the texture is there to diffuse light, and Fictiv rates polycarbonate higher on matte than Hubs does, so B-1 or B-2 is the steadier pick in our reading.

Beyond SPI: etched pattern textures

Leather, wood-grain and similar patterns are not SPI grades; Protolabs describes Mold-Tech textures as applied after the cavity is milled, by chemical etching for light textures or by a 5-axis laser for more complex ones. For these the draft is set by texture depth, and the published rates differ. Xometry asks for an extra 1.5° per thousandth of an inch of texture depth and lists MT-11030, 0.002 in deep, at 3°. Protolabs recommends “one degree of draft for every 0.0005 in. to 0.0006 in. (0.0127mm to 0.01524mm) of texture depth,” or “roughly 6 to 7 degrees for a typical wood grain or leather-like finish,” and notes that “Some textures may reach depths of 0.003 in. (0.0762mm) or more.” At that 0.003 in depth the Xometry rate adds 1.5 × 3 = 4.5°, while the Protolabs rate gives 0.003 ÷ 0.0006 = 5.0° up to 0.003 ÷ 0.0005 = 6.0°. When you know the etch depth, the draft angle calculator adds the texture allowance to a base angle and works out the dimension change; this page stops at naming the floor.

Common mistakes

  • One finish note for the whole part. Protolabs points out that different finishes “can be applied to the A and B sides of the mold.” Call the cosmetic face and leave the hidden faces non-cosmetic.
  • Choosing gloss for a part that will be handled. Xometry credits matte faces with helping against fingerprints on handled products. Weigh that before you settle on an A grade for a grip or a lid.
  • Picking texture after the draft is frozen. A blasted or etched face can need several degrees more than the wall was designed with. Choose the finish first, then set the draft.
  • Asking for a deep finish inside narrow ribs. Protolabs says “finishes on deep and thin ribs may not be possible on parts as they are challenging to reach within the mold.”
  • Using Ra as the grade. Ra figures sit beside SPI grades in some tables, but the grades are defined by method. Use the surface roughness converter for Ra, and the grade name on the drawing.
  • Expecting a later touch-up. Protolabs notes that the finish is applied to the mold and transferred in molding, so “secondary finishing is not available, which makes material selection critical in some cases.” Pick resin and finish together.

Where this selector fits among other routes

RouteGood forWhere it falls short
This selectorNaming a grade early, checking a resin against a look, seeing whether the draft can carry a textureReads one published rating table and three draft figures; knows nothing about your color batch or tool steel
Draft angle calculatorExact draft and dimension change once the texture depth is knownDoes not pick the finish
Surface roughness converterRa, Rz and grade-number conversionsRoughness alone does not describe the look
A physical finish reference agreed with the toolmakerPinning down what a grade name means before the cavity is finishedIt is not your part, your resin or your color
First molded shots in the real compoundThe final cosmetic sign-offComes after the tool exists
From the tooling floor: mark the finish on the part drawing face by face, with the seen faces shaded and the grade written beside each, and put “non-cosmetic” against the rest. A single title-block line that says one grade everywhere leaves the toolmaker guessing which faces deserve the hand work, and the guess may not match yours.

Sources for the method

All eight pages listed were read in full on November 20, 2026. The SPI finish standard document itself is not quoted here; the grade descriptions come from the public reproductions listed.

Reviewed by the JCH tooling team · updated November 2026.

SPI finish questions

In a finish callout like B-2, what do the letter and the number stand for?

The letter tells you what touched the steel last, and the digit tells you how fine that abrasive was. In the A family a diamond compound buffs the cavity, in B it is grit paper, in C an abrasive stone, and in D the face is dry blasted. Inside A, B and C the digit 1 marks the finest grit and 3 the coarsest. In D the 1 is a glass-bead satin blast, while 2 and 3 use oxide grits that leave a dull and then a rough face. B-2 is therefore the middle paper grade of the semi-glossy family.

Which SPI grade should a see-through window or lens get?

Xometry lists A-1 against optically clear work and A-2 against transparent parts, and keeps A-3 for lenses that are not optical. It also notes that clear parts typically get the polish on both mold halves, not only the show side. Resin narrows the choice: Protolabs Network gives acrylic its top mark on every diamond grade, while polycarbonate scores only Average at A-1 and Good at A-2.

How much more draft does a textured mold face need than a polished one?

Protolabs sets a 3 degree minimum for its light bead-blast finish, PM-T1, and a 5 degree minimum for its medium bead blast, PM-T2. For its buffed, sanded and stoned finishes it states no extra figure. Treating SPI D-1 like PM-T1 and D-2 or D-3 like PM-T2 is our reading; none of the SPI tables we found print a draft angle.

Why should polycarbonate stay away from the D-2 and D-3 finishes?

Fictiv says plainly to avoid that pairing, and the Protolabs Network table marks polycarbonate Not recommended on both oxide blasts and on the two coarser stone grades, C-2 and C-3. Yet the same table gives polycarbonate Excellent on the glass-bead D-1 blast. Neither page explains the reason, so take it as a published rating to respect, not a mechanism we can vouch for.

Can a polished finish survive glass or mineral filler in the resin?

It can. Protolabs warns that glass and mineral fillers may streak and can make one polish grade hard to tell from the next on the molded part. Its own comparison: an unfilled nylon picks up finishes more than a nylon with 30% glass fill. On a textured face, glass fibers may read as stringy or sparkly. Approve the cosmetic grade on a shot of the real compound.

If my drawing names no finish, what will the mold faces get?

The two guides answer slightly different questions. Fictiv says that for molds needing none of the twelve finishes, the SPI standard specifies an as-machined face with visible machining marks, while Xometry says that, unless otherwise specified, a molded part will “typically have an SPI B-2 default finish”. Either way, write a grade or the words non-cosmetic against each face of the drawing so nobody has to guess.

Is the Ra figure next to each SPI grade part of the standard?

Protolabs Network and Fictiv print a typical Ra range beside every grade, but the grades themselves are defined by abrasive and method, and two of them, A-3 and B-1, carry the same printed range while looking different. This selector does not use Ra to choose a grade. For roughness numbers and unit conversion, the surface roughness converter is the place.

Ask JCH about a finish

Torn between two grades, or unsure how a filler or a color changes the call? Type the question below. Ask JCH is software, not a person: its answer appears in a chat window, and once it has answered, an optional email box appears for a follow-up.

Replies come from an AI model and may be wrong; check anything that matters against a molded sample.

A look in mind and a resin that fights it?

Send the model and tell us which faces a customer sees. Our tooling team will mark a grade on each face, point out walls whose draft is too shallow for the texture you want, and suggest a resin swap where the published ratings say the pairing is weak.

Book a free 30-minute first consultation Send the model and the faces that show
JCH Design & Manufacturing — tooling, injection molding, PCBA, custom packaging, cut-and-sew & QC via vetted partner factories · Book a 30-minute call · jack@jchtrade.com · (321) 323-4474 · Canonical: https://jchtrade.com/tools/spi-finish-selector