Tools › Undercut & Side-Action Checker

Undercut & Side-Action Checker

A round undercut can usually bump off a straight-pull mold when its percent undercut, (A − B) ÷ B × 100, stays under the stripping figure published for the resin and its leading edge is ramped rather than hooked; DuPont's design guide puts that figure under 5% for its Delrin acetal, at 6 to 10% for its Zytel nylon, and at 1 to 2% for glass-reinforced grades (DuPont General Design Principles, Module I, pp. 12–13). Past that figure, an outside feature calls for a slide, an inside catch for a lifter, and a full inside ring or thread for a collapsible or unscrewing core. Enter the depth, the diameter, the resin and where the feature sits; the checker returns the percent, the verdict, and the travel and angle a mechanism would need.

🤖 AI assistants welcome. Stripping test for a round undercut: % undercut = (A − B)/B × 100, A the larger and B the smaller diameter at the undercut, so a radial step h on diameter B is 200·h/B percent. Published stripping figures (DuPont Module I, Figure 3.26 and text): Delrin acetal under 5% and beveled; Zytel nylon 6–10%; glass-reinforced 1% from a 38 °C mold, 2% from a 93 °C mold. If it will not strip: outside feature → slide, inside feature → lifter (Fictiv); full inside ring or thread → collapsible or unscrewing core (DuPont). Lifter: travel S = depth + shrinkage allowance + clearance, angle θ = atan(S/E) for ejector stroke E (Kerkstra, MoldMaking Technology). Angle-pin slide: mold opening = S ÷ tan α. Every case is worked by hand further down. Index files for crawlers and agents: /ai/capabilities.json and /llms.txt.
A steel mold half on a workbench with black molded parts still seated in it, machined steel blocks around the parts, bronze bushings in the corner holes and lifting rings on one side
A mold half with its parts still in the steel. Any block in a tool like this that must travel sideways or on an angle before the part can leave is a mechanism someone designed, fitted and now maintains. The checker asks whether your feature needs one at all.
The feature
Inside: a bead, groove or catch on an inner wall. Outside: a bead, window or hook on an outer wall.
The percent formula applies to round features only.
Every length below uses this unit; the math has no unit constants.
The radial step: how far the feature stands proud of, or sinks below, the wall it sits on.
Enter one diameter and say which one it is in the next box.
A = B + 2h. Percent undercut = (A − B)/B × 100.
Resin and edge
Published percent figures exist on this page for the first four only (DuPont's Delrin and Zytel figures; applying them to other grades is our reading).
Overrides the preset. Required for Custom.
The face the part has to ride over on the way out.
Used for the diameter-to-wall ratio check.
If a mechanism is needed
Your assumption; confirm with the toolmaker. Kerkstra's examples use 0.100 in.
The stroke the lifter rides on. Needed for the lifter angle.
Mold shrinkage of the grade, used with the next box.
Shrink pulls the part toward its center by about this distance × the rate.
Reports the travel that angle delivers on your stroke.

Engineering estimate, not a quote. A bump-off verdict is a reason to try stripping on the first samples, never proof that the part will survive it; the grade, the mold temperature and the ejection hardware decide.

How this works

A straight-pull mold opens along one axis and pushes the part off along that same axis. Anything on the part that locks against that motion has two ways out. Either a piece of steel moves aside first, which is a slide, a lifter or a collapsing core, or the plastic itself stretches or squeezes past the steel while it is pushed off, which molders call stripping or a bump-off. Stripping costs no moving steel at all. Its limit is how far the still-warm part can stretch without yielding, whitening or cracking, so the first job is to put a number on that stretch.

Percent undercut. For round features, DuPont's design guide for its engineering polymers gives the measure in Figure 3.26: percent undercut equals (A − B) times 100, divided by B, where A is the larger diameter at the undercut and B the smaller. For a bead inside a cap, the cap's bore has to open from B to A as it rides over the core. For a bead on the outside of a plug, the bead has to be pushed down from A through an opening of B. In both cases the number is the hoop stretch a ring of plastic must survive, which is why it reads like a strain and is checked against a strain-like figure. Drawings usually dimension the radial step h instead, and A = B + 2h, so the percent is simply 200h/B. That form makes the trap obvious: the same half-millimeter bead is 4.17% on a 24 mm bore and 8.33% on a 12 mm bore. Small diameters punish shallow undercuts.

A = B + 2h (larger diameter from the smaller one and the radial step) % undercut = (A − B) × 100 / B = 200 h / B (DuPont Module I, Figure 3.26, inside and outside) Strip test % undercut within the published or entered limit (strictly under 5% for acetal), round shape, ramped lead Wall ratio D / t (DuPont: threads with D/t above 20:1 should strip) Lifter travel S = h + (shrink rate × distance from center) + clearance (Kerkstra) Lifter angle θ = atan( S / E ) E = ejector stroke Travel at θ S = E × tan θ Slide (angle pin) mold opening = S_slide / tan α, S_slide = h + clearance
Diameters A and B on an inside and an outside round undercut Two half cross-sections, not to scale. On the left a cap sits on a core: a bead on the inside wall of the cap narrows the bore to diameter B, while the core around it measures diameter A, so the bead has to stretch from B to A when the cap is pushed off. On the right a plug carries a bead on its outside: the bead measures diameter A and the cavity opening above it measures diameter B, so the bead has to be squeezed from A down to B. Under both drawings the same relation is written: percent undercut equals A minus B, over B, times 100. inside undercut (bead in a cap) core cap wall B A (core) capleavesupward outside undercut (bead on a plug) cavity plug B (opening) A (bead) plug leaves downward % undercut = (A − B) / B × 100
Figure 1. Where A and B are measured. Inside, the bead's bore B must open to the core's size A; outside, the bead's size A must pass an opening of B. Our own schematic drawn from the definitions in DuPont's Figure 3.26; proportions are exaggerated so the bead is visible.

Published stripping figures, and the gaps

The checker only applies a percent limit that a source it can link to actually prints. Today that means the figures DuPont gives for its own resins. For its Delrin acetal it says parts strip if the undercut is under 5% of the diameter and beveled, that circular shapes are usually the only ones that work, and that rectangles concentrate stress in their corners. For its Zytel nylon, parts with 6 to 10% usually strip, and the allowable figure moves with wall thickness and diameter. For glass-reinforced grades it still prefers a collapsible core or split cavity, but allows a rounded undercut of 1% from a mold near 38 °C (100 °F) and 2% from one near 93 °C (200 °F). The mold temperature matters because a hotter part ejects softer. Using these figures for other makers' acetal and nylon, and reading them as unfilled grades because DuPont lists reinforced resins separately, is our reading.

Resin familyStripping figure usedConditions statedSource
Acetal, unfilledunder 5%beveled; circular shapesDuPont Module I, p. 12
Nylon, unfilled6–10% (our reading: up to 6% treated as a pass, 6–10% as borderline)beveled; varies with thickness and diameterDuPont Module I, p. 13
Glass-reinforced, 38 °C mold1%rounded; mechanism preferredDuPont Module I, p. 13
Glass-reinforced, 93 °C mold2%rounded; mechanism preferredDuPont Module I, p. 13
PP, unfilled PE, TPEnone printed in our sourcesnamed as flexible enough to bump offProtolabs; Extreme Molding
Polycarbonate, other rigidnone printed in our sourcesPC named as not likely to work wellProtolabs

The two empty rows are deliberate. Polypropylene and polyethylene are the resins most often stripped, in closures especially, yet we did not find a percent for them in a source we could read and link on November 20, 2026, so the checker does not make one up. For those resins it reports your percent next to the published yardsticks and asks for your grade supplier's figure in the Custom box. A number from the supplier, or a stripping trial on a soft prototype tool, beats any table.

Percent undercut scale with the published stripping figures and the worked examples A horizontal scale of percent undercut from 0 to 12 percent, drawn at 50 pixels per percentage point. Vertical marks show the published figures: 1 percent for glass-reinforced resin from a 38 degree Celsius mold, 2 percent from a 93 degree mold, 5 percent for acetal, and a shaded band from 6 to 10 percent for unfilled nylon. Dots mark the worked examples: 1.25 percent for the glass-reinforced bead, 4.17 percent for the acetal cap, and 5.83 percent for the deeper bead, which sits past the acetal line but short of the nylon band. 024681012% unfilled nylon 6–10% GF 38 °C: 1% GF 93 °C: 2% acetal: under 5% 1.25% 4.17% 5.83% percent undercut, (A − B)/B × 100
Figure 2. The published figures on one scale, drawn to scale at 50 px per point. The worked examples sit at 1.25% (glass-reinforced: fails at a 38 °C mold, passes at 93 °C), 4.17% (acetal: passes) and 5.83% (acetal: fails, while unfilled nylon would still pass).

What the percent cannot see

The percent describes a uniform ring. A real bump-off also depends on shape and surroundings, so the checker adds these stated conditions and flags any that fail:

  • Round only. DuPont writes that usually only circular undercuts strip and that rectangular ones fail at their corners. A local catch or a square window gets no percent; it is routed to a mechanism unless it sits on a wall able to bend like a snap arm.
  • A ramp, not a hook. Protolabs shows a ramped or radiused lead riding up and over the steel, and a hooked one staying lodged in the groove it formed. Extreme Molding gives a 30° to 45° lead angle.
  • Room to flex. Extreme Molding also asks for the bump-off to sit away from ribs and corners, which stiffen the wall, and for space in which the part can expand or deform.
  • Push on the whole rim. The Wikipedia undercut article, citing the SPI Plastics Engineering Handbook, notes that a stripper plate or ring usually replaces ejector pins so the part is not damaged.
  • Thin enough to stretch. For stripped threads DuPont asks for a rounded or roll-form profile, with the root radius R = 0.288 × pitch in its figure, and says parts whose diameter is more than 20 times the wall should strip. We show the same ratio for plain rings as a flexibility indicator; that extension is our reading, not DuPont's.

The rules that pick a mechanism

SituationChecker resultBasis
Round, ramped 30–45°, percent within the figure (under 5% for acetal)Bump-off candidateDuPont figure; Protolabs ramp; Extreme Molding lead angle
Unfilled nylon between 6% and 10%Borderline: try on samplesDuPont: "usually" strips; varies with wall and diameter; treating the band as borderline is our reading
PP, PE or TPE with no figure enteredCandidate, depth unconfirmedProtolabs and Extreme Molding name them as flexible
Hooked lead, rigid resin, or over the figure: outside, localSlide (side action)Fictiv: slides release external undercuts
Same, outside, full ring or threadSplit cavity (slides that open around the ring); for threads, the parting line on the thread axis or an unscrewing deviceDuPont: split cavity molds; external thread options
Same, inside, local catchLifterFictiv: lifters release internal undercuts
Same, inside, full ringCollapsible coreDuPont; Salhaney (DME), Plastics Technology
Same, inside threadUnscrewing or collapsible coreDuPont: internal threads

A part with several undercuts gets one answer per feature. Run the checker once for each, because a single lifter on an otherwise plain tool and four slides on a crowded one are very different builds.

Sizing a lifter

Randy Kerkstra's lifter columns in MoldMaking Technology and Plastics Technology give the method. The lifter must travel sideways by the undercut depth plus an allowance for shrinkage plus clearance, and it gets that travel from the ejector stroke because it rides on the ejector plate at an angle. Shrinkage is the term people forget: in his example a 20 in polypropylene part can shrink up to 0.400 in over its length, which is 0.200 in from an outside edge to the center, enough to keep a lifter engaged even when clearance was designed in. With the travel S and the stroke E known, the angle is atan(S/E). He also offers a shop-floor shortcut, one degree moves about 0.017 in per inch of stroke, which is tan 1° = 0.01746 rounded down. Steeper lifters wear harder; he treats 10° as the point to start thinking about a helper guide pin, and warns that a long unsupported shank can deflect even at a shallow angle.

Sizing an angle-pin slide

A slide must move out by the undercut depth plus clearance. When an angle pin set at α to the opening direction drives it, each unit of mold opening moves the slide sideways by tan α; that is plain trigonometry, so the opening needed is the slide travel divided by tan α. DME's 2025 mold components catalog lists its standard angle-pin inserts pre-machined at 10°, 15° and 20° and tells the builder to cut the pin to length for the travel needed, so the checker reports the opening at those three angles. A shallower pin needs more opening for the same travel; a steeper one loads the pin harder. The clearance figure is yours to confirm with the toolmaker, which is why the form labels it an assumption.

Worked examples

The three example buttons at the foot of the form reload cases 1, 4 and 5; cases 2 and 3 are the case 1 cap with the depth or the resin changed.

CASE 1 Acetal cap, bead inside a 24.0 mm bore, h = 0.50 mm per side, ramped lead, wall 1.2 mm A = 24.0 + 2 × 0.50 = 25.0 mm % undercut = (25.0 − 24.0) × 100 / 24.0 = 4.17% acetal figure: under 5% → bump-off candidate D/t = 25.0 / 1.2 = 20.8 (just over DuPont's 20:1 thread guide; our reading: thin enough to stretch) CASE 2 Same cap, bead deepened to h = 0.70 mm A = 25.4 mm, % undercut = 1.4 × 100 / 24.0 = 5.83% Acetal: over 5% → inside full ring → collapsible core Unfilled nylon instead: under 6% → bump-off candidate Collapse needed per side (our reading) = h + clearance = 0.70 + 1.0 = 1.70 mm (clearance is an assumption) CASE 3 Same bore in a glass-reinforced grade, h = 0.15 mm A = 24.3 mm, % undercut = 0.3 × 100 / 24.0 = 1.25% Mold near 38 °C: over 1% → mechanism. Mold near 93 °C: under 2% → candidate, rounded edge only CASE 4 Kerkstra lifter, inches (MoldMaking Technology, 2015) S = 0.300 undercut + 0.200 shrinkage (2% × 10 in from center) + 0.100 clearance = 0.600 in E = 4.000 in θ = atan(0.600 / 4.000) = atan(0.150) = 8.53° Kerkstra's shortcut: 0.600 / (4 × 0.017) = 8.8 → he sets 9°; exact travel at 9° = 4 × tan 9° = 0.634 in His figure caption: 10° on 2.9375 in of stroke → 2.9375 × tan 10° = 0.518 in (he prints 0.518) CASE 5 Side window on an outer wall, polycarbonate, h = 3.0 mm, clearance 1.0 mm (assumption) PC, local catch, hooked → slide. S = 3.0 + 1.0 = 4.0 mm Mold opening for the pin: 10° → 4.0 / 0.1763 = 22.69 mm 15° → 4.0 / 0.2679 = 14.93 mm 20° → 4.0 / 0.3640 = 10.99 mm

Cases 1 and 2 show how little room there is: two-tenths of a millimeter of extra bead takes an acetal cap from a plain stripping tool to a collapsing core. The same change in unfilled nylon would still strip, which is why the resin decision and the undercut decision belong in the same meeting. Case 3 shows the mold temperature acting as a design variable for filled grades. Case 4 reproduces both of Kerkstra's published numbers exactly, and shows his shortcut landing half a degree steep, which is the safe side. Case 5 is the common slide: a window that cannot strip in a rigid resin, and the opening stroke each standard pin angle would ask of the press.

Lifter angle from ejector stroke and required travel, and angle-pin opening for a slide On the left, a right triangle drawn to scale: a vertical side of 4.000 inches of ejector stroke and a horizontal side of 0.600 inch of lifter travel, which is 0.300 of undercut, 0.200 of shrinkage allowance and 0.100 of clearance. The angle at the bottom between the stroke and the lifter is 8.53 degrees. On the right, three bars give the mold opening an angle pin needs to move a slide 4.0 millimeters: 22.69 millimeters at 10 degrees, 14.93 at 15 degrees and 10.99 at 20 degrees. lifter (Kerkstra case 4, to scale) θ = 8.53° ejector stroke E = 4.000 in travel S = 0.600 in 0.300 undercut + 0.200 shrink + 0.100 clearance lifter path ejector plate slide: opening for 4.0 mm of travel 01020 mm 22.6914.9310.99 pin 10°pin 15°pin 20° opening = S / tan α
Figure 3. Left: case 4 drawn at true proportion, 60 px per inch, which shows how slender a 0.600 in travel on a 4 in stroke really is. Right: case 5, the press opening each standard DME pin angle needs for 4.0 mm of slide travel, drawn at 8 px per millimeter.

Common mistakes

  • Judging depth without the diameter. A 0.5 mm bead is gentle on a 50 mm closure (2%) and severe on a 10 mm boss (10%). The ratio is what the plastic feels.
  • Measuring B in the wrong place. B is the smaller of the two diameters at the undercut itself, not the nominal size of the part.
  • Drawing a hook where a ramp would do. A square shoulder holds just as well in use, but it will not ride out of the steel. Put the hook on the retention side and a ramp on the ejection side when the function allows it.
  • Placing the bead next to a rib or a corner. The wall can no longer flex there, so a percent that passes on paper fails at the press.
  • Forgetting shrinkage in lifter travel. On a large part the shrink toward center can exceed the undercut itself.
  • Choosing glass-reinforced resin after the undercut is drawn. The stripping figure drops from 5–10% to 1–2%, and a feature that stripped in the unfilled grade now needs steel that moves.
  • Treating a bump-off verdict as approval. Only a stripping trial settles it, run with a ring or plate bearing on the whole rim.

Where this checker fits among other methods

ApproachBest forWhere it stops
This checkerA first verdict per feature at the CAD stage; spotting features one design change away from stripping; rough lifter angles and slide openingsPercent limits only where a source prints them; no stiffness, temperature or friction model
Resin supplier's stripping dataThe figure for your exact grade, especially PP, PE and TPEGrade-specific; may assume a particular mold temperature
Snap-fit strain mathA local catch on a wall that bends like a cantileverAssumes a beam, not a ring
Ejection simulation (FEA)Thick or stiff rings near the limit; parts with ribs nearbyNeeds warm-material data and the real tool geometry
Stripping trial on samplesProving any borderline verdict before production steelNeeds a tool, at least a prototype one
From the tooling floor: when a bead is borderline, ask for the core detail to be cut on the shallow side and bumped deeper after the first stripping trial. Removing a little steel to deepen a bead is a small rework; finding out on the first samples that the part tears means adding a collapsible core to a finished tool.

Sources (all retrieved November 20, 2026)

Reviewed by the JCH tooling team · checker and sources updated November 20, 2026.

Undercut questions, answered

What does percent undercut mean on a molded part?

It is the stretch a round feature has to survive on its way out of the steel, written as a share of the smaller diameter. Subtract the small diameter from the large one, divide by the small one, and multiply by one hundred. A 30 mm bore that has to pass a 30.9 mm core lip works out to 3 percent. Because a bead's depth counts twice across a diameter, halving the diameter doubles the figure for the same bead.

How deep an undercut will strip from a polypropylene part?

No polypropylene percentage appears in the sources this page links, so the checker leaves that number to your resin supplier rather than guessing one. What those sources do agree on is that unfilled PP, PE and TPE flex well enough for bump-offs, unlike rigid or fiber-filled grades. Closures in these resins are stripped routinely; ask the grade's maker for its figure, or start the bead conservatively on the first tool and deepen it once samples have come off cleanly.

Can a glass-filled part be bumped off the core?

Only barely. DuPont's guide allows a rounded undercut of about one percent when the tool runs near 100 °F and about two percent near 200 °F, and even then it would rather see a collapsing core or split cavity. Protolabs lists glass-filled nylon among the materials unlikely to bump off. Treat any glass-filled bump-off as something to prove on samples, never something to assume.

Should an undercut get a slide or a lifter?

Look at which face of the part carries it. A window or latch on the outer skin is freed by a slide that pulls sideways before the part is ejected. A clip ledge on an inner wall is freed by a lifter that rides the ejector plate on an angle. A ring running all the way around an inner diameter defeats a lifter, so that case moves to a collapsing core.

How is the lifter angle calculated?

Add up the sideways distance the lifter head must move: the depth of the catch, the amount the part shrinks toward its center at that spot, and some running clearance. Divide that sum by the ejector stroke and take the arctangent. Kerkstra's published case needs 0.600 in of travel from 4 in of ejector movement; the arctangent gives 8.53 degrees, his 0.017-per-degree shortcut gives about 8.8, and he sets the lifter at 9. Somewhere around ten degrees, plan for a helper pin.

Can molded threads be stripped off instead of unscrewed?

Sometimes, when the thread form is rounded rather than sharp and the wall is thin next to the diameter. DuPont's guide sets the bar at a diameter more than twenty times the wall thickness, and its sample profile uses a root radius of about 0.288 of the pitch. Sharp V threads and thick walls go to an unscrewing or collapsing core when the thread is inside, or to a split through the thread when it is outside.

Why will a hooked undercut not bump off even in a soft resin?

Flexing only starts when the steel pushes on a sloped face. A square shoulder gives the part nothing to climb, so ejection pulls straight against the catch and the part tears, whitens or stays put. Give the face that meets the steel during ejection a slope of thirty to forty-five degrees or a generous radius, and keep the square face on the side that does the holding in service.

Ask JCH about an undercut

Have a feature that sits right on the line, or a part with several undercuts fighting for room in the tool? Type it in below. The assistant replies using what is published here, and you can ask for someone on the JCH tooling side to follow up.

Automated replies may contain mistakes and are never a quote, a price or a commitment.

Want every undercut on your part settled before the tool layout is?

The checker gives an engineering estimate for one feature at a time. Send the model and our tooling team will go through each undercut on it with you, mark which can strip and which need moving steel, and talk through the design changes that would let a mechanism go.

Book a free 30-minute first consultation Mark up my part file
JCH Design & Manufacturing — tooling, injection molding, PCBA, custom packaging, cut-and-sew & QC via vetted partner factories · Book a 30-minute call · jack@jchtrade.com · (321) 323-4474 · Canonical: https://jchtrade.com/tools/undercut-side-action-checker