Answers › Joining molded parts

What are the ways to join two molded plastic parts?

Reviewed by the JCH tooling team · Updated

Snap fits and screws come apart; welding fuses parts of the same or compatible resin; heat staking melts a plastic stud over a second part of any material; adhesives bond dissimilar materials. Pick by whether it must open, whether the resins match, whether it must seal, and the part's size, then design the joint features into the mold.

There are three families of joints for molded parts. Mechanical joints (snap fits, screws, press fits) can be undone, at least in principle. Welds (ultrasonic, vibration, hot plate, spin) melt the two parts into one and need compatible plastics. Staking and adhesives sit in between: staking melts a plastic stud over a second part, which can be metal or a circuit board, and adhesives bond almost anything at the cost of surface prep and cure. The right method follows from four questions, and every one of them changes the part design.

The options side by side

MethodComes apart?MaterialsWhat it asks of the part
Snap fitOftenAny flexible enough gradeHook arms, strain limits, a way for the mold to form the undercut
ScrewsYesAny; inserts for frequent serviceBosses, gussets, sink control
Ultrasonic weldingNoSame or compatible resinsEnergy director or shear joint, alignment, joint near the horn
Vibration weldingNoSame or compatible resins, larger partsJoint flange in one plane of motion, flash traps, room for melt-down
Hot plate weldingNoSame resin, non-symmetric or fragile assembliesWide, flat joint flange; even walls
Spin weldingNoSame resin, round jointsCircular joint and a drive feature for the spinning half
Heat or ultrasonic stakingNoPlastic stud through any second materialMolded studs sized to the head you want
Adhesive or solventNoDissimilar materials, large shapesLap or tongue-and-groove joint, glue gap, surface prep

Four questions that pick the method

  1. Must it come apart for service or recycling? Then snaps or screws; see snap-fit design and screw boss design.
  2. Are both parts the same plastic? Welding needs compatible resins. Branson's ultrasonic guide states that compatibility exists only among amorphous polymers and blends, and that semi-crystalline polymers weld only to themselves.
  3. Must it seal? Welds and adhesives can seal; snaps and screws need a gasket. See sealed enclosures.
  4. How big, what shape, and what is inside? Small parts with electronics suit ultrasonic welding or staking; large parts suit vibration welding; round joints suit spin welding; DuPont recommends hot plate welding for non-symmetric parts with fragile internals that can't take vibration.

Ultrasonic welding

A horn vibrates one part against the other, friction heats the joint, and the plastic melts and fuses under pressure. BASF puts typical weld time at about 0.5 to 1.0 second on 20 kHz equipment, with 40 kHz machines used for small, delicate parts. Almost everything depends on the joint design.

For amorphous resins such as ABS, the standard joint is a butt joint with an energy director, a small triangular ridge molded on one face. Dukane's design guide sizes its base at 20–25% of the wall thickness (W/4 to W/5). For amorphous resins it is a 90° triangle, so the height is half the base; for polycarbonate, acrylic and semi-crystalline resins Dukane uses a sharper 60° triangle, 0.866 times the base in height. Its overall size range is about 0.13–0.76 mm high and 0.25–1.5 mm wide. Branson adds that the parts need their own alignment features, and that ejector pins must stay out of the weld area.

Semi-crystalline resins such as nylon and acetal melt sharply and refreeze before the melt from an energy director can flow across, so BASF and Branson recommend a shear joint: the lid telescopes into the base with a small interference, and the melt smears along the vertical walls. Dukane calls the joint near-field when it is 6.4 mm (¼ in) or less from the horn contact; farther away, energy is lost on the way, especially in semi-crystalline resins.

Two ultrasonic weld joints: a butt joint with a triangular energy director for amorphous resins, and a shear joint with interference for semi-crystalline resins A. Energy director (amorphous) top part bottom part wall W base W/4 to W/5 90° apex: height = base/2 60° apex for PC, acrylic, semi-crystalline small first contact melts fast and flows across the joint B. Shear joint (semi-crystalline) lid interference per side fixture supports the walls lid telescopes in; melt smears along the vertical walls

Worked example: sizing three joints

Energy director on an ABS housing. The wall at the joint is 2.0 mm. Base width W/4 to W/5 = 0.40 to 0.50 mm; use 0.45 mm. ABS is amorphous, so the apex is 90° and the height is 0.45 ÷ 2 = 0.23 mm, inside Dukane's range. Were the housing polycarbonate, the 60° form would make it 0.866 × 0.45 = 0.39 mm tall.

Shear joint on a nylon lid, 60 mm across. Branson's table puts parts from 38 to 76 mm at 0.36–0.46 mm interference per side, with a part tolerance of ±0.075 mm, and asks for at least 2.0 mm of wall on the bottom part so it doesn't buckle. Branson's table stops at 76 mm; beyond that it suggests an energy director instead. Nylon absorbs moisture, so Dukane says to weld right after molding or bag the parts with desiccant.

Heat stake holding a circuit board. A 3.0 mm molded stud passes through a 1.6 mm board. Branson's high-profile dome stake suits bosses of 6.35 mm (0.250 in) or less: stud height = board thickness + 1.75 × stud diameter = 1.6 + 5.25 = 6.85 mm, giving a head about 2 × 3.0 = 6.0 mm across and 0.75 × 3.0 = 2.25 mm tall. For studs of 4 mm (0.156 in) and up, Branson's hollow stake melts less plastic, avoids sink on the far face, and can later take a self-tapping screw if the board must come out.

Mold opened between the tie bars of an injection molding machine: a bare-steel half on the left, a blue-painted half on the right, no part in the tool
An empty mold opened on an injection molding machine. Molded parts leave a press like this before any joining step; the photo shows only the machine and tooling.

Vibration, hot plate and spin welding

Vibration welding rubs the parts together at a lower frequency and larger stroke than ultrasonic welding. BASF gives 120 Hz or 240 Hz machines with peak-to-peak amplitudes of about 1.5–3.6 mm and 0.8–1.7 mm respectively, weld times of 2 to 3 seconds and a melt-down of 0.38–0.76 mm. The motion has to happen in one plane, so the joint flange must lie in that plane (it can be gently curved), and the side walls need fixture support so they don't flex. Flash traps beside the joint hide the squeezed-out melt.

Hot plate welding melts both faces on a heated platen and then presses them together. DuPont recommends a joint width at least 2.5 times the wall, flat joint faces and even walls. It warns that nylon generally oxidizes on the plate; dry-as-molded nylon can be welded, but moisture can cut weld strength by up to 50%, and glass fiber, which does not cross the joint, can cut it by up to 50% too. Spin welding, per DuPont, spins one round part against the other until a melt film forms, then stops and holds, producing a strong, stress-free joint.

Adhesives and solvents

Adhesives join dissimilar materials and large or awkward shapes. DuPont's Delrin guide notes bonded joints are strongest in compression and shear and comparatively weak in peel, cleavage and tension, so design overlapping lap or tongue-and-groove joints rather than butt joints. BASF lists the trade-offs by family: epoxies are strong and heat resistant but poor in impact and slow to cure; cyanoacrylates cure in seconds but are limited to about 93 °C (200 °F) and have limited moisture resistance; silicones seal and flex but are weak. Low-energy resins are hard to bond: acetal needs etching or roughening, and the solvent that cements it is expensive and toxic. Solvent welding suits amorphous resins with a known solvent and parts you can ventilate.

What goes wrong

Common questions

What is the strongest way to join two plastic parts?

A well-designed weld between compatible resins usually comes closest to the strength of the parent plastic, and DuPont reports vibration welds approaching it. The joint design, moisture and glass content all matter: DuPont notes that moisture or glass fiber can each cut a hot plate weld in nylon by up to half.

Can two different plastics be welded together?

Only if they are compatible. Branson's design guide says compatibility exists among some amorphous polymers and blends, while semi-crystalline polymers weld only to themselves. For other pairs, use staking, adhesives, snaps, screws or a two-material molding process instead.

What is an energy director?

A small triangular ridge molded onto one face of an ultrasonic weld joint. Its point melts first, so the weld starts quickly and the melt flows across the joint. Dukane sizes the base at a quarter to a fifth of the wall thickness, with a 90 degree apex for amorphous resins and 60 degrees for others.

When should I use heat staking instead of welding?

When the part being held is a different material, such as a circuit board, metal bracket or label plate, that cannot be welded to the plastic. A molded stud passes through a hole in that part and is melted into a head. It is permanent, quick and needs no fasteners.

Do I need to design the joint before the mold is made?

Yes. Energy directors, shear-joint steps, staking studs, snap hooks, screw bosses and flash traps are all molded features. Adding them later means cutting or welding mold steel. Decide the joining method during the design review so the features are in the tool from the first shot.

Sources

Send the part file and the quantity you expect to run, and we'll review it before you commit to tooling. NDA first if you want one.