Up to 25 percent clean regrind of the same grade is the common published ceiling. UL accepts it for listed parts without retesting, and several resin makers recommend the same limit. Many parts should use less or none: medical, clear, color-critical and highly loaded parts often specify virgin only. How the regrind is ground, dried and controlled matters as much as the percentage.

What counts as regrind

Regrind is plastic that has already been through the press once, usually sprues and runners from a cold-runner tool plus start-up and rejected parts, chopped in a granulator and fed back into the hopper with new pellets. UL's description, drawn from its UL 746D standard, is narrow on purpose: reclaimed scrap from molding, such as sprues or runners, reused at the molding facility that made it. Once that material leaves the molder, UL treats it as recycled plastic instead, because its history can no longer be traced.

That definition is the key to the whole question. Clean regrind of the same grade, from the same press, ground and dried properly, behaves almost like virgin resin. Mixed, wet, contaminated or repeatedly cycled material does not.

What the standards and resin makers actually allow

SourceWhat it says
UL Solutions, on UL 746DRegrind meeting the definition can make up to 25% of the hopper feed, with the other 75% being the same virgin grade the parts came from.
Celanese, Vectra LCP design guideLimit regrind to 25% to keep color and mechanical properties; UL accepts up to 25% for parts under a UL listing without further testing. Some grades are approved at 50%, one at 75%. The processor sets the upper limit case by case.
Lubrizol, Isoplast processing guideUp to 25% regrind if contamination and moisture pickup are avoided. Parts rejected because they were molded wet must not be reground.

So "up to 25%" is the common default in published guidance, not a law of physics. It is a ceiling chosen so that the old material stays a small minority. Whether your part can use 25%, 10% or none is a spec decision, made with the resin supplier's data and testing of the real part.

Why a limit exists: heat history

Every pass through the barrel adds heat and shear. Celanese lists four ways regrind loses properties: contamination, thermal decomposition, hydrolysis (reaction with water) and damage to reinforcing fibers, which shortens glass and can cut notched impact strength. One lab study, published in Polymers in 2020, shows why a single test can mislead. It reground 100% of a polypropylene five times on an ultrasonic micro-molding machine, which is not a normal screw press, so its numbers do not transfer to a production blend. Even so, the pattern is worth knowing: weight-average molecular weight fell by 48% from the raw pellet and zero-shear viscosity dropped from about 12,000 to about 1,100 Pa·s, while tensile strength held up or even rose until the fifth pass. A quick tensile check can pass while the chains are getting shorter. A melt flow comparison against virgin is the cheaper early warning.

Worked example: where the old material goes

Assume a cold-runner tool where regrind is fed back at a steady rate, and the regrind itself contains the mix from earlier shots. In each shot the virgin share has been melted once; the regrind share carries everything older. At a constant fraction r, the share melted k times works out to (1 - r) x r^(k-1).

Share of a shot that has been melted once, twice, three times or more, at a steady 25 percent and 50 percent regrind rate How many times has the plastic in one shot been melted?25% regrind50% regrind75%50%25% 1st melt (virgin) 2nd melt 3rd melt 4th melt 5th melt or more Steady state, regrind fed back at a constant rate. At 50% the old-material tail is about 16 times larger than at 25% (6.25% vs 0.39% at five melts or more).

Doubling the regrind rate from 25% to 50% raises the second-melt share only from 18.75% to 25%, but it makes the five-plus tail about sixteen times bigger. That tail is the material most likely to be degraded, discolored or full of fines. It is why resin makers and buyers draw lines at modest levels, and why a molder that quietly runs 50% regrind is a different supplier from one that holds 15%.

Injection mold clamped closed in a press, with blue clamp blocks and steel tie bars around it
A mold running in the press. On a cold-runner tool every cycle also makes a sprue and runner, and how that scrap is ground, dried and blended back decides whether regrind helps or hurts the part.

Grinding and drying matter as much as the percentage

When the answer is zero

Many specs ban regrind outright. Common cases are medical and food-contact parts where traceability and material history matter (see food-safe and medical molding), clear optical parts where any specks or yellowing show (see clear parts), safety-critical or highly loaded parts, and parts whose color must match lot to lot, covered in color matching. Hot-runner tools make the question smaller in the first place, since there is no cold runner to grind; the hot vs cold runner note explains that trade.

How to write it into your spec

  1. State the maximum regrind percentage by weight, or "virgin only."
  2. Require regrind to come only from the same part, grade and color, from runners and start-up scrap, never from field returns or rejected parts molded wet.
  3. Require the same drying as virgin, and a closed, labeled container between granulator and hopper.
  4. Ask how the ratio is controlled: a proportioning loader with a set ratio is checkable; a bucket by the hopper is not.
  5. Approve first articles at the regrind level used in production, not at 0% then switch. A switch changes color, flow and weight.
  6. For critical parts, ask for a melt flow check on blended material against the virgin value as an early warning of degradation.

Regrind policy also belongs in quality and inspection plans, and the cost side of using it, versus paying for a hot runner, is a normal cost-down discussion. The part weight calculator helps estimate how much runner scrap a design generates per shot.

Common questions

Is regrind the same as recycled plastic?

No. Regrind is a molder's own clean scrap, such as runners and start-up parts, reground and reused at the same plant with the same grade. Recycled plastic comes from outside that loop, either post-industrial or post-consumer, and its history is unknown. UL treats the two differently for that reason, and specs should too.

Does regrind always reduce strength?

Not always in a way a simple test shows. Each melt shortens polymer chains and can break glass fibers, but tensile strength may hold up while toughness, impact and long-term properties fall. At modest levels of clean, dry regrind the change is often small. The risk rises with high percentages, poor drying and contamination.

Can I use regrind on a medical or food-contact part?

Often the answer is no, because the regulatory file, the customer spec or the resin supplier's medical-grade terms call for virgin material with full lot traceability. Where regrind is allowed, it is usually tightly limited and documented. Check the device or food-contact requirements before allowing any regrind.

Why does regrind change the color of my parts?

Material that has been melted more than once can yellow or darken, and regrind from a different color or lot shifts the shade. Changing the ratio from shot to shot also changes the color. Celanese limits regrind to 25 percent partly to keep color uniform, and color-critical parts often specify a fixed ratio or none.

How do I know my supplier is following the regrind limit?

Ask how the ratio is set and checked. A proportioning loader with a recorded setting, labeled regrind bins kept with each job, and records of material lots are good signs. Approve first articles at the production ratio, and include regrind control in factory audits and the quality agreement.