Use masterbatch when one natural resin runs in several colors and the molder doses accurately, typically about 2 to 5%. Use precolored compound for tight brand colors, heavy pigment loads or short runs, since nothing is dosed at the press. Use liquid color for tints and low doses, if the molder runs it routinely.
Almost every colored molded part gets its color in one of three ways. The difference that matters most is where the mixing happens and who controls the dose.
Pellets packed with pigment in a carrier resin, metered into natural resin at the press. A trade article on coloring polymers puts typical let-down ratios at 20:1 to 50:1, natural resin to masterbatch, which is roughly 5% down to 2%. Colorant makers also offer concentrates designed for lower doses; one supplier case study cites 1 to 3% for a concentrate used across several different resins. The concentrates themselves are heavily loaded: in one colorant maker's molding catalog, many white masterbatches carry 60 or 70% titanium dioxide, and the blacks range from under 20% up to 60% carbon black.
The resin maker or a compounder melts pigment into the resin on a compounding extruder, usually twin-screw for high pigment loads, and ships pellets that are already the final color. Nothing is dosed at the press. The color is fixed before the resin arrives.
Pigment dispersed in a liquid carrier, pumped into the feed throat from a drum or pail through a pickup lance. Liquid is commonly used for tinted clear and translucent parts and for opaque parts at let-down ratios under 2%, and it disperses well.
| Masterbatch | Precolored compound | Liquid color | |
|---|---|---|---|
| Who controls the color dose | The molder's doser, every shot | The compounder, once per lot | The molder's pump, every shot |
| Typical dose | about 2 to 5%; some grades 1 to 3% | none at the press | often under 2% |
| Shot-to-shot consistency | Good with gravimetric dosing; drifts if pellets separate in the hopper | Best; nothing to drift at the press | Good when the pump is maintained; stops without warning when the container runs dry |
| Hard colors and high pigment loads | Can be difficult or uneconomic | Best fit | Possible; screw slip risk at higher doses |
| Switching colors | Easy; one natural resin, several concentrates | Separate resin inventory per color | Easy, but purging and cleanup take care |
| Relative material cost | Middle | Usually highest per kilogram, but can win on short runs through less setup and scrap | Lowest colorant use per part |
| Shop-floor headaches | Dosing calibration | Very few | Spills, screw staining, shelf life, separation, cold-weather freezing |
The precolored-on-short-runs point surprises people. A trade article on medical device coloring notes that precolored polymers can save setup time and raise part acceptance rates enough to save money on short runs, even though the pellets cost more. When a short run means a long tuning session at the press, the extra per-kilogram cost is often the cheaper option.

A hypothetical two-cavity mold makes a 60 g part per cavity with an 8 g cold runner: 128 g per shot. The color is a mid-blue masterbatch specified at 2% of the total blend.
Now compare a precolored version of the same blue. There's no step 3, 4 or 5: every pellet carries the same color, and the variation comes down to the compounder's lot control, which is checked once per lot instead of once per shot. If the blue is a brand color under a tight ΔE limit and the run is modest, that's a strong argument for precolor. If the same part runs in six colors from one natural resin, masterbatch wins on inventory.
If the part is going to be painted, printed or labeled anyway, the molded-in color may only need to be close, and the cheapest adequate method wins; pad printing and silk-screen decoration covers that route. If the order quantity is small, a precolored compound may come with its own minimum per color from the compounder, which can change the math; compare it against the run sizes discussed in minimum order quantities. And if material cost per part is the driver, the cost per part calculator shows how much the colorant actually adds compared with resin, cycle time and scrap.
It is how much color concentrate is mixed into natural resin. A 50:1 ratio means 50 parts natural resin to 1 part masterbatch, about 2%. Trade sources put typical masterbatch ratios at 20:1 to 50:1, roughly 5% to 2%, and some concentrates are made to run at 1 to 3%.
Usually, yes. The pigment is compounded into every pellet before shipping, so nothing at the press can change the dose. Masterbatch depends on the molder's doser and on concentrate pellets not separating from the natural resin in the hopper. Good gravimetric dosing closes much of the gap.
Liquid color typically runs at lower let-down ratios than pellet concentrates, often under 2% for opaque parts, so less colorant goes into each part. The savings can be offset by pump equipment, cleanup, shelf life and handling issues, which is why many molders standardize on pellets instead.
It can, especially at higher doses or with an incompatible carrier resin. The carrier resin dilutes the base resin. At typical doses with a compatible carrier the effect is usually small, but a load-bearing or rated part should be tested in its production color, not in natural.
It depends on the color tolerance and run size. For a single brand color with a tight tolerance and modest volume, precolored compound often gets to approved parts fastest. For a part that will run in several colors, masterbatch keeps one natural resin in stock. Approve color on molded parts either way.
Send the part file and the quantity you expect to run, and we'll review it before you commit to tooling. NDA first if you want one.
Send a part for reviewBook a 30-minute call